Use any ni base electrode like ENiCrMo3 for this weld, before welding do backing at 250 deg cel min for 30 min then maintain 150 deg cel during welding interpass must be contoll at 300 deg cel max
After welding cover with blanket to reach room temp at uniform rate of cooling
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
Subscribe to:
Post Comments (Atom)
Re: [MW:35686] HDPE WPS
Refer ASME SEC IX There is separate chapter for Plastic welding . Based on that you have to prepare Sent from my iPhone On 21 Jun 2025, at...
-
Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? ...
-
Definition of buttering from ASME Section IX, QW/QB-492 Definitions: Buttering: the addition of material, by welding, on one or bot...
-
Section I. PRINT READING 3-1. GENERAL a. Drawings . Drawing or sketching is a universal language used to convey all necessary information to...
No comments:
Post a Comment