If you are confident, yes, you can do the repair work. For machinable
weld, you can use:

1.    98 Ni (+)2 fe - (AWS/SFA  E Ni-CI)
2.    55 Ni (+) 45 Fe - (AWS/SFA  ENi-Fe-CI)
3.    65Ni (+)4Fe (+) 30Cu - (AWS/SFA- Ni-Cu B)

Pre-heat to 75- 100 deg. C to remove oil, grease, rust, paint strains and
use above electrodes. If you use any other LH electrode like E 7016,
preheat  should be on higher side (say 350deg. C) and have to maintain
inter pass temperature and slow cooling rate.

Not worried about colour matching  and chemistry try with E 308
(or) E 309. With its high ductility, these electrodes may help you at times. 

Sridhar.
---------------------------------------------------------------------------

On Saturday 6 January 2018, 10:28:06 AM IST, Mikko Laine <maikeydii@gmail.com> wrote:


Boxbe This message is eligible for Automatic Cleanup! (maikeydii@gmail.com) Add cleanup rule | More info
Hello,

we have an old machine part with two 28 mm keyway slots ground out due wear. We need to fill up those key ways and machine new slots but due to construction limitations any other methods such as machining a replacement bore insert are not suitable.

Slots are approximately 36mm wide, 7mm deep and 140 mm long. The bore diameter where they are located is around 140mm. So far we have received mixed opinions on weldability of this material: one slight "yes might be doable with correct procedure" and two "DO NOT WELD IN ANY CASE!!!"...


So do any of you have good guidance on suitable welding procedure for cast steel GS-45?
Best regards,
Mikko Laine

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...