Re: [MW:21300] diferrence between E7018.. OK 55 & E7018.. OK 48

OK 48 is E 7018 and is with Mn up to 1.2% 
The impact strength is 80 J at  -40 C.  UTS  values are app. 540 N/sq.mm.
Works win DCEP, DCEN & AC 90 OCV.
 
OK 55 is E 7018-1 and is with Mn up to 1.5% 
The impact strength is 80 J at  -50 C.   UTS values are app. 590 N/sq.mm.
Works with only DCEP & AC 65 OCV t
U will get the values after a prolonged PWHT.

As U have seen, impact strength is higher in OK 55 and recommended 
where more impact is needed.

The baking temp. weld ability is same except that, u will  end up paying 
bit more for OK 55.There is no necessity to change to OK 55 when not needed. 


Regards,
C Sridhar.
Technical Adviser - Welding,
for Alsta Pristine Engineering Private Limited, --(SS fab).  Bangalore

(A venture of Advance Eng. Training & Inspection Services). Chennai,

Mobile nos: 0 94449 71097, 0 7406 326326, 0 94445 21267. 

From: Mahesh Unninarayanan <mahesh84kumar@gmail.com>
To: materials-welding@googlegroups.com
Sent: Thursday, 26 June 2014 7:36 PM
Subject: [MW:21268] diferrence between E7018.. OK 55 & E7018.. OK 48

Dear all,

Was there any difference in the weld quality if we  use one with E7018.. OK 55 and other with E7018.. OK 48..
Is there any  difference in temperature range for baking and holding  between the above two.. kindly share your information regarding this.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.


No comments:

[MW:35668] Selection of Filler/Electrode.

Dear Gentlemen, Kindly advise me as we have tube to tubesheet joint. Tube moc is incoloy 800 And tubesheet moc is F53 SDSS (Super duplex sta...