Re: [MW:21217] Preheat for 10025 S355

Hello,
 
As per the BS EN 1011-2, there is two type of way for calculation,
 
1) As per the BS EN 1011-2 Annex C, Method A.
 
Reference figure- C.2b of BS EN 1011-2
Example :-
 
Combined thickness -31.25 mm
Heat Input -3.61 KJ/mm ( Maximum heat input as per the calculation)
Hydrogen scale-  D (as per table c.2 and used consumable) (Hydrogen Scale Value is mentioned in MTC of consumable)
Carbon equivalent -0.433 (assumed as per the raw Material MTC used for PQR)
 
Minimum preheat temperature- 0deg C ( As per figure #C.2.a of BS EN 1011-2)
 
2) Calculation of the preheat temperature.
 
Tp= 697*CET+160*tanh(d/35)+62*HD power 0.35+ (53*CET-32)*Q-328
 
In your cash pre heat temp will be 0degC
 
 

Regards,
ANAND. B. HIREMATH


On Sat, Jun 21, 2014 at 4:45 PM, <rexrecede2012@gmail.com> wrote:
Dear Experts,

Is there someone can help me how much preheat temperature required for BS 10025 S355JR thickness 8-25mm based on BS5135 or EN 1011-2. I'm planning to use e6010/e7010 for root pass and e7018 for filling and capping.

Regards,

Jhared Rhecede
QC Inspector

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...