[MW:18461] Re: 18451] CVN Test Temperature Reduction AWS D1.1

Dear all.! Good day.!

   For the above case the test temperature would be :  -20-11.1= -31.1 deg C 

  My query is base metal thickness to be considered in temperature reduction ( code reference please )
 
  For example, if the material thickness is 7mm and specimen is 10X4mm, MDMT -20 deg C , the test temp would be..?  (-36.8 or -32.3 deg C - code reference please )

Note: ASME sec VIII Div 1,  it is clearly mentioned that the base metal thickness to be considered , Para UG 84 (c) 5 (b)



On Saturday, 17 August 2013 12:48:42 UTC+3, duc hoang wrote:

Dear

 

The temp is -31.1OC

 

Thanks & Regards

Hoang Van Duc

QC site

Gorgon Heavy Lift and Tie In project

(+84)0943266655

 

From: material...@googlegroups.com [mailto:material...@googlegroups.com] On Behalf Of nguyen anh tuan
Sent: 17 August, 2013 3:36 PM
To: material...@googlegroups.com
Subject: [MW:18451] CVN Test Temperature Reduction AWS D1.1

 

Dear Experts

 

I have question about using sub-sized specimen for CVN test

Testing temperature following specification   is -20oc ,Plate thickness is 8mm and specimen sized is 10x5

My question How much temperature will apply for testing (AWS D1.1)

 

"4.36.7 When sub-sized specimens are required, and the

width of the specimen across the notch is less than 80%

of the base metal thickness, the test temperature shall be

reduced in conformance with Table 4.15, unless otherwise

specified in the contract documents

Thanks in advance

 

 

Tuan

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

No comments:

[MW:35668] Selection of Filler/Electrode.

Dear Gentlemen, Kindly advise me as we have tube to tubesheet joint. Tube moc is incoloy 800 And tubesheet moc is F53 SDSS (Super duplex sta...