Re: [MW:16396] Stress Relieving heat treatment of Monel 400


Mr.Sanjay,

Welded MONEL alloy 400 components normally go into service as welded. If there is a concern that the
environment could induce stress corrosion cracking (e.g, steam containing ammonia), the structure could
be stress relieved by heat treatment at 620 0 C to 760 0 C. It could be done by using LPG pumping,
Electrical Resistance heating, Furnace  etc.

Sridhar
.
------------------------------------------------------------------------------------------------------------------------------------------------------------------


From:
Rajagopal Kannan <rajagopal.kannan@gmail.com>
To: "materials-welding@googlegroups.com" <materials-welding@googlegroups.com>
Sent: Monday, 31 December 2012 3:49 PM
Subject: Re: [MW:16392] Stress Relieving heat treatment of Monel 400

Dear Sanjay,
As per UNF 56 of ASME sec. VIII Div.1, UNS N 04400 is not required to be Post Weld Heat treated.
Thanks and Best Regards,
K.Rajagopal


On Tue, Jun 1, 2010 at 3:16 PM, Sanjay Gandhi <sanjayseju88@gmail.com> wrote:
Hi,
 
Has any body come across requirement of PWHT or stress relieving for Monel 400? I have read some where that Monel 400 material that is to be used in HF acid service, welds must be given stress reliving treatment to minimize the risk of stress corrosion cracking. 
 
I am looking for following information.
1.) Whether post weld heat treatment is necessary for welds of Monel 400 operating in HF service. Any precedence of heat treatment or no heat treatment?
2.) If heat treatment is inevitable, how to carry out heat treatment of complete vessel? Conventional way by heating or any new technique, any specific furnace, any inert gas to be used, etc…
3.) Any cleaning treatment required after heat treatment? What is the effective method of cleaning?  
 
I would highly appreciate your inputs on the above. We have got two Monel 400 vessels to be used in HF services.
 
 
Regards,
 
Sanjay Gandhi
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 


No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...