Re: [MW:16370] Temp. reduction in sub size specimen for Charpy impact test

Dear Farhang,
The laboratory was right. You can refer the appendix of A333 which made an example for these cases. Totally the 3C reduction is right.

Regards

On Sat, Dec 29, 2012 at 10:47 AM, Farhang <hyperm2m@gmail.com> wrote:

Dear All

I need to know way of calculation temperature reduction when we use sub size specimen.

My problem:

I have tested an A333 Gr.6 (4" pipe-6.3 mm thickness). Labratoary used a sub size specimen (55*5*10). and they tested it in -48c. test temperature of A 333 Gr.6 is -45C and they tested it in 3c cooler temperature Unfortunately absorbed energy was low and my test failed.

But i see a clause in standard(SA-333/SA-333M) which described that:

" 14.1.2) When sub size Charpy impact specimens are used and the width along the notch is less than 80% of the actual wall thickness of the original material "

Is this clause applicable for my case??????

Really i don't know which one is correct?
  • (5/6.3) * 100 = 79% then i should not apply the above mentioned clause and i shall calculate reduction temperature and test my sample in cooler temperature(-45-3=-48).
  • (10/6.3) * 100 = 159% then i should not apply the above mentioned clause and no need to reduction temperature and test my sample in MDMT(-45).

** In the above text i use different color for digits because you can trace them easier.


Many Thanks
Farhang

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 



--
M. Shokri Arfaei
International Welding Engineer (IWE)
ASNT NDT Level III
ISA - STRI - Metallurgy Lab. Manager
Tel: +98-21-66282127
Fax: +98-21-66282779
 
Please don't print this e-mail unless you really need to. BeGreen!

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

No comments:

[MW:35633] IP Joint

Hello experts, I would like to know what is IP joints in piping(31.3)?  Regards Saurabh -- https://materials-welding.blogspot.com/...