Tuesday, April 21, 2009

[MW:1998] Fw: [MW:1995] Re: WELDER QUALIFICATION

Dear Mr. Jones,

Your interpretation seems to be more appropriate. QW 423.1 may be
applicable over and above QW 301.2. Thanks
for the update, anyway.

Best regards,

Prasad

Dale Jones
<dalejones7978@ya
hoo.com> To
Sent by: materials-welding@googlegroups.com
materials-welding cc
@googlegroups.com
Subject
[MW:1979] Re: WELDER QUALIFICATION
18/04/09 07:02 AM


Please respond to
materials-welding
@googlegroups.com

QW-423.1 clearly states "base metal used for welder qualification may be

substituted for the metal specified in the WPS in accordance with the

following table." That table allows the welder to weld P1 material

together with F5 filler while following a P8 qualified procedure.


Regards,


Dale Jones


--- On Fri, 4/17/09, pjoshi@technip.com <pjoshi@technip.com> wrote:


From: pjoshi@technip.com <pjoshi@technip.com>

Subject: [MW:1973] Re: WELDER QUALIFICATION

To: materials-welding@googlegroups.com

Date: Friday, April 17, 2009, 3:16 AM

Dear all,


I would like to add a point here. So far as I understand, you need to use

a

qualified procedure for welded qualification as well (Refer QW 301.2). In

this situation, you cannot use any hypothetical WPS (like, P1#P1/F5)

unless

otherwise you qualify the same accordingly. I remember we had qualified

such procedure once and for all when I was WE at L&T Hazira Works.


Best regards,


Prasad


BHARAT GOLE


<bharatgole@hotma


il.com>

To

Sent by: material welding


materials-welding <

materials-welding@googlegroups.com

@googlegroups.com >

cc


17/04/09 10:18 AM

Subject

[MW:1971] Re: WELDER QUALIFICATION

Please respond to


materials-welding


@googlegroups.com


Mr. Dale Jones

As you said to weld with F5 stainless steel filler material which is

needed

to weld with matching filler on P8 materials.I would like to add

more...i.e. as per QW 423 Alternate Base Materials for welder

qualification

we can weld P1 materiel also with F5 SS Filler in order to qualify

welder

for any particular P8 WPS.

This is economical as well as within limit of code.

Please correct me if my interpretation is wrong

Regards


Bharat B. Gole

Date: Thu, 16 Apr 2009 16:26:34 -0700

From: dalejones7978@yahoo.com

Subject: [MW:1970] Re: WELDER QUALIFICATION

To: materials-welding@googlegroups.com


This is correct that the welder can weld on all of these materials but do


not ignore the other variables. For example the welder will be restricted


to the Fnumber filler material he qualified with. An example is a SMAW


qualification. When a welder qualifies on P1 material with a matching F4


SMAW filler he will be qualified to the base material range stated below


and with F1-F4 carbon steel filler material. This will not qualify him to


weld with F5 stainless steel filler material which is needed to weld with


matching filler on P8 materials. The same concept will apply to various


other P numberd materials. To fully understand this concept and the other


variables that will restrict a welders qualifications, read article 3 and


QW-416 in ASME Section 9

Regards,

Dale Jones

--- On Thu, 4/16/09, Muhammed Ibrahim <ibratech@gmail.com> wrote:

From: Muhammed Ibrahim <ibratech@gmail.com>


Subject: [MW:1968] Re: WELDER QUALIFICATION


To: materials-welding@googlegroups.com


Date: Thursday, April 16, 2009, 5:45 AM

Not only P11. Also P34 & P41 thru P49. The reason is, the skill of the


welder required to weld any of these material is same. So he can proove


it in any one P No. mentioned .

Regards,


Muhammed Ibrahim


2009/4/16 gaurav mongia <er.gauravmongia@gmail.com>

IF A WELDER IS QUALIFIED FOR P1 material and in code it is

written

that he is qualified upto P11.

i wanna know what will be reason that a welder can do welding on


all


material upto P11 instead he is only qualified in P1

How fun is this? IMing with Windows Live Messenger just got better.


Save a tree...please don't print this e-mail unless you really need to.

Save a tree...please don't print this e-mail unless you really need to.

This email and any attached files ("Message") may contain confidential

and/or privileged information. It is intended solely for the

addressee(s). If you receive this Message in error, inform the sender by

reply email, delete the Message and destroy any printed copy.

Any unauthorized use, distribution, or copying of this Message or any

part thereof is prohibited. Emails are susceptible to alteration. Neither

Technip nor any of its affiliates shall be liable for the Message if

altered or falsified nor shall they be liable for any damage caused by

any virus that might be transmitted with this Message.

Save a tree...please don't print this e-mail unless you really need to.

Save a tree...please don't print this e-mail unless you really need to.


This email and any attached files ("Message") may contain confidential
and/or privileged information. It is intended solely for the addressee(s).
If you receive this Message in error, inform the sender by reply email,
delete the Message and destroy any printed copy.
Any unauthorized use, distribution, or copying of this Message or any part
thereof is prohibited. Emails are susceptible to alteration. Neither
Technip nor any of its affiliates shall be liable for the Message if
altered or falsified nor shall they be liable for any damage caused by any
virus that might be transmitted with this Message.

Save a tree...please don't print this e-mail unless you really need to.

Save a tree...please don't print this e-mail unless you really need to.




This email and any attached files ("Message") may contain confidential and/or privileged information. It is intended solely for the addressee(s). If you receive this Message in error, inform the sender by reply email, delete the Message and destroy any printed copy.
Any unauthorized use, distribution, or copying of this Message or any part thereof is prohibited. Emails are susceptible to alteration. Neither Technip nor any of its affiliates shall be liable for the Message if altered or falsified nor shall they be liable for any damage caused by any virus that might be transmitted with this Message.


--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

No comments:

[MW:35668] Selection of Filler/Electrode.

Dear Gentlemen, Kindly advise me as we have tube to tubesheet joint. Tube moc is incoloy 800 And tubesheet moc is F53 SDSS (Super duplex sta...