Skip to main content

Posts

Re: [MW:23011] HOLDING OF ELECTRODES

Dear all,  As it's knows the  coating of Low Hydrogen Electrodes (basic electrodes) include CaCO3 and CaF2(Calcium Fluoride),ferroalloys (ferrosillicium, ferromaganese) and iron powder. I would like to open a discussion about  the arc(DCEN,DCEP) stability (effect of the CaF2,CaCo3 content of coating): -the arc stability evaluated by conductivity of the arc gap B (B=I/Ut where I,U and T are respectively the current(A) Voltage(V)and ignition time(sec)of the arc.) -CaCo3/CaF2 ratio influence of arc stability -since the slag of these electrodes contain SiO2 and TiO2 oxides .melting of the electrodes has as result intensive interacation of these oxides with CaF2 with formation of gaseous with influence of arc stability. Could somebody provide more explanation/infos concerning the above subjects? GIGI ZEGHEANU EWE - TOTAL E&P From: pgoswami <pgoswami@quickclic.net> To: materials-welding@googlegroups.com Cc: mechsivachidambaram@gmail.com Sent: Sunday, 29 ...

RE: [MW:23010] HOLDING OF ELECTRODES

Mr. Sivachidambaram, Please see the attached document for your guidance. If these electrodes are in " hermetically sealed" packs, one may avoid rebaking. There is no specific time limits for storage @ 150 Deg C, however storing for months would not be advisable. You need to go with your electrode manufacture's recommendations. Thanks. Pradip Goswami, P.Eng,IWE Welding & Metallurgical Specialist Ontario, Canada pgoswami@quickclic.net pradip.goswami@gmail.com http://ca.linkedin.com/pub/pradip-goswami/5/985/299 -----Original Message----- From: materials-welding@googlegroups.com [mailto: materials-welding@googlegroups.com ] On Behalf Of safad pp Sent: Sunday, March 29, 2015 2:12 AM To: materials-welding@googlegroups.com Subject: Re: [MW:23009] HOLDING OF ELECTRODES Dear SIvachidambaram, You can keep it for continuously @ 150 deg . Before that theses electrodes shall be baked @ 250-300 deg for 2 ...

Re: [MW:23009] HOLDING OF ELECTRODES

Dear SIvachidambaram, You can keep it for continuously @ 150 deg . Before that theses electrodes shall be baked @ 250-300 deg for 2 hours .Once should we take care that, the required quantities of electrodes should be taken for baking ,then long time holding can be avoided . And also when baked electrodes contact with room temp for more than 4 hours ,then again re-bake required . Shafad P.P CSWIP3.1 /AWS -CWI On Sun, Mar 29, 2015 at 10:51 AM, Siva Chidambaram < mechsivachidambaram@gmail.com > wrote: > Hi Friends, > > Can anybody guide me that how long shall i keep Low Hydrogen electrode on a > Holding oven at a temperature of 150deg Cel. > > > Regards, > M. SIvachidambaram > > -- > You received this message because you are subscribed to the Google Groups > "Materials & Welding" group. > To unsubscribe from this group and stop receiving emails from it, send an...

[MW:23008] HOLDING OF ELECTRODES

Hi Friends,   Can anybody guide me that how long shall i keep Low Hydrogen electrode on a Holding oven at a temperature of 150deg Cel.     Regards, M. SIvachidambaram -- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To post to this group, send email to materials-welding@googlegroups.com . Visit this group at http://groups.google.com/group/materials-welding . To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAPJQpMVuWcr205AurnK7pcGORGKDSRon_cMDXQ9uTndK7C4ivA%40mail.gmail.com . For more options, visit https://groups.google.com/d/optout .

Re: [MW:23006] Welding filler wire/Electrod for A 105 to A335 P11

Dear Friends, You can use Er 70S-2 for root welding by TIG process and E7018 for fill passes by ARC process. Pre heat and PWHT to be maintained for P11 conditions( ie: P no 4 conditions as per ASME sec VIII Div 1) Regards, Sankaran.Sp Welding & Metallurgy expert      On Tuesday, 24 March 2015 12:36 PM, Bala Murugan <balamuruga2003@gmail.com> wrote: ER80S- B2 + E8018 B2 On Mar 24, 2015 11:42 AM, "Bala Murugan" < balamuruga2003@gmail.com > wrote: You may use E 8018 B2 On Mar 24, 2015 11:09 AM, "B Osare" < bosare@nfl.co.in > wrote: Dear Experts,   Can any one suggest the suitable welding filler wire and electrode for welding CS A105 to A335 P11.   Regards   B Osare N F L Vijaipur   From: Harikrishnan N S Sent: Monday, March 23, 2015 2:13 PM To: materials-welding@googlegroups.com Subject: [MW: 22996] Re: 20405] ASME Sect IX-QW-405-Position Qualification Ranges [GroupMai...

[MW:23006] Re: 4140 & 4130 material

Preheating is a must for these materials, because of carbon content (nearl %0,40) 300 C preheating is necessary and low cooling rate. After welding it's better to use pwht (normalizing) ER80S-B2 - (CrMo1), E8018-B2 (CrMo1) can be used or some of dissimilar consumables, such as ER307 (18 8 Mn), ER312 (29 9) Best regards. Murat 27 Mart 2015 Cuma 04:37:55 UTC+2 tarihinde Pravin yazdı: Dear experts, Kindly advice which welding consumable should I select for following material: 1. 4140 SMAW,GTAW,FCAW,SAW 2. 4130 SMAW GTAW FCAW SAW Since above listed both material are high tensile material, is there any special heat treatment or welding condition need to be taken into consideration for better mechanical result. Kindly advice Pravin Singapore Sent from my iPhone -- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an ...

[MW:23005] 4140 & 4130 material

Dear experts, Kindly advice which welding consumable should I select for following material: 1. 4140 SMAW,GTAW,FCAW,SAW 2. 4130 SMAW GTAW FCAW SAW Since above listed both material are high tensile material, is there any special heat treatment or welding condition need to be taken into consideration for better mechanical result. Kindly advice Pravin Singapore Sent from my iPhone -- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To post to this group, send email to materials-welding@googlegroups.com . Visit this group at http://groups.google.com/group/materials-welding . To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/6633E2BE-FC71-4C50-9F7A-30344D9EF19E%40gmail.com . For more options, visit https://groups.googl...