Re: [MW:22008] WELDING JOINT A335 P91

Dear experts, As per my expereince, we should use B9 instead of B3. During operation (One year) it will give type III or IV crack and we need to cut it out again. According to Babcock and Wilcox and Vallaourec & Mannesmann, it might give higher hardness and we may do not get the required micro structure as well.  Kind regards Muhammad Hussain Lead Metallurgist TCR Arabia Company Limited Dammam- Saudi Arabia  On Sunday, September 28, 2014 11:29 AM, Bala Nechur <bala.Nechur@phoenixindustrial.ca> wrote: Hello Expert,   I recommend to use ER9S-B9 and E9018-B9 which will match the chemistry of A335 Gr P91 material.   Bala Nechur, Corporate QA/QC Manager Phoenix Industrial, Office: 780-428-3130  Ext 736 Cell: 780-204-0239 Fax: 1-866-211-3193 Toll Free: 1-866-778-3130 Email: bala.nechur@phoenixindustrial.ca              ...

[MW:22005] Re: QW 406 , preheat maintenance

Dear Sir, Preheat maintenance, according to ASME IX,  is not post heating . If it should be carried out NDT or not sure welding joint perfect, you can cool down before PWHT. Preheat maintenance means that you do not cool down before perform PWHT On Friday, June 20, 2014 7:29:50 PM UTC+7, rajesh s. mhaske ,Engineer Welding ,PUNE,INDIA wrote:    Dear sir                thickness and  OD : 323 od* 70 mm thk                welding process : GTAW+SMAW                Material : SA106 Gr B                Preheating : 100 deg c                weld deposition : for GTAW : 4 mm, SMAW : 66 mm    Question  :   ...

RE: [MW:22005] WELDING JOINT A335 P91

Hello Expert,   I recommend to use ER9S-B9 and E9018-B9 which will match the chemistry of A335 Gr P91 material.   Bala Nechur, Corporate QA/QC Manager Phoenix Industrial, Office: 780-428-3130  Ext 736 Cell: 780-204-0239 Fax: 1-866-211-3193 Toll Free: 1-866-778-3130 Email: bala.nechur@phoenixindustrial.ca                                                                                                       The information transmitted is intended only f...

Re: [MW:22007] Welder qualification

Dear Mohit,   F Number is an essential variable for welders qualification. If the F-No used in the CS does not cover that to be used for the Overlay as per QW-433 , then the welder is not qualified to perform such overlay. In any case, you will also need to consider the requirement of QW-381.3.   Dear Mahendra,   When a chemical composition is stipulated in the WPS, it simple implies that every weld performed must meet the stipulated chemical composition and chemical analysis of the production weld may be required by spot check. It is then a requirement that every welder must be qualified using that particular WPS and strickly following the weld parameters as stipulated in the WPS.   Regards,   Rems Okonkwo IWE Nigeria On Fri, Sep 26, 2014 at 7:26 PM, Mohit Aggarwal < aggarwalmohit05@gmail.com > wrote: Dear Sir, Thanks for your reply. Code is ASME section IX.and consumable is E309LMo. My query is sir if a welder is qualified in CS Groove weld then h...

[MW:22004] WELDING JOINT A335 P91

Dear Experts, We have study case, on our project (steam power plant project), there was any welding joint i.e. welding pipe A335 P91 to A335 P91 with filler metal GTAW ER90S-B3 + SMAW E9015-B9 and PWHT 750 C with holding time 2 hours . Please advise us, what impact these welding joint for strength and lifetime if compare with GTAW ER90S-B9 + SMAW E9015-B9 and PWHT 750 C with holding time 2 hours . What can we do and the solution this case. Thanks and regards Winarko QA/QC Welding Inspector +6281288300094 -- To post to this group, send email to materials-welding@googlegroups.com To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com For more options, visit this group's bolg at http://materials-welding.blogspot.com/ http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm   The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users...

Re: [MW:22002] Welder qualification

Hello rems Discussing to QW-381.3 , how  chemical composition affects on welder qualification....what if we write the chemical composition in the WPS and qualify welder by following this clause... This clause is not having clarity.. can you do us a favour by giving little more clarification on this.... Regards Mahendra arya On 26-Sep-2014 11:04 pm, "Rems Okonkwo" < rems.okonkwo@gmail.com > wrote: Dear Mohit,   Although your query lack all necessary information like the applicable code, the type of consumable, materials etc but on a general note, welders qualified for clad restoration are not qualified to weld butt joints but when a welder is qualified on butt weld, the weld is qualified to weld clad restoration if only   1. requirement for Chemical composition.   2. within the F number of the consumable qualified,   3. within the welding position qualified   Please refer to ASME IX Art III (See Below)   QW-381.3 Alternative Qualificat...

Re: [MW:22003] Welder qualification

Dear Sir, Thanks for your reply. Code is ASME section IX.and consumable is E309LMo. My query is sir if a welder is qualified in CS Groove weld then how he can qualify for overlay as overlay is always done by Inconel or SS whatever it is!! Best Regards, Mohit Aggarwal. On 26-Sep-2014 11:04 PM, "Rems Okonkwo" < rems.okonkwo@gmail.com > wrote: Dear Mohit,   Although your query lack all necessary information like the applicable code, the type of consumable, materials etc but on a general note, welders qualified for clad restoration are not qualified to weld butt joints but when a welder is qualified on butt weld, the weld is qualified to weld clad restoration if only   1. requirement for Chemical composition.   2. within the F number of the consumable qualified,   3. within the welding position qualified   Please refer to ASME IX Art III (See Below)   QW-381.3 Alternative Qualification With Groove Weld Tests. When a chemical composition...