Skip to main content

Posts

[MW:12565] HARDNESS MEASUREMENT MAP

Dear Experts, We have completed sucessfully Hydrotest of our two SS 316L vessles.  For stress relieiving reasons, we have asked our supplier and since the beginning, to foresee some spot checks on hardness of the shells. Now, is there any standard mapping/ number of points to be checked?? Logically, the more strained fiber is by the external surface of the shell, so which points to select or hardness testing?? Many thanks for a prompt reply Regards, -- Meilleures salutations Mokrani Lassaad 00216 20 649 755 http://www.linkedin.com/pub/lassaad-mokrani/16/364/907 P     Pensez environnement! N'imprimez ce mail que si c'est vraiment nécessaire Please consider your environmental responsibility before printing this e-mail This e-mail is confidential and it is intended only for the addressees. Any review, dissemination, distribution, or copying of this message by persons or entities other than the intended recipient is prohibited. If you have received this e-mail in error, kindly...

[MW:12564] RE: 12563] PWHT of modified P460 NL1 (1.8915) EN 10028-3

Dear Sir,   I don't know what ASME says about PWHT but in the EN 10028-3 there is a warning about PWHT for this material regarding holding time and/or temperature (see paragraph 8.2.4 of EN 10028-3). When the outcome of following formula comes above 17,3 there is a risk that the material properties will be reduced and no longer met the requirements of the specification.   P = T s (20 + lg t ) x 10 -3   Where Ts = PWHT temperature in °K and t is holding time in hours   If your outcome is above this 17,3 than you need to prove that all mechanical properties still meet the requirements by simulating PWHT on a sample from the same heat and thickness as used for your pressure vessel. When executing more than one PWHT than you should calculate the value for each separate treatment and look at the sum of all treatments together. Keeping this formula in mind you also can calculate any possible heat treatment conditions (temperature for thickness of 14,3 max. 630 °C)   M...

[MW:12561] RE: 12548] defect on circ-seam of H2 service vessel

Hello Hrishi,   The attached picture is not very clear. However looking at the problem I would think there could be two scenarios:- Devise a plan for smooth grinding and blending of the notch to the surrounding base metal.Ensure that minimum design metal thickness+required corrosion allowance is maintained, upon discussion with the design engineer. If the above option is not acceptable then you may resort to controlled heat input weld deposition technique as per API-510, 8.1.6.4.2.3 Controlled-deposition Welding Method (Notch Toughness Testing Required). It would be advisable to  to qualify weld repair procedure as per Sec-IX, QW-290 with hardness control and preferably with impact test(if the original design specification calls for so). The temper bead weld repair, is a substitute for PWHT if the above guidelines are followed. Once the qualified welding procedure is used for weld repair, required NDE follo...

[MW:12563] PWHT of modified P460 NL1 (1.8915) EN 10028-3

As this material is not in the tables can anyone provide the PWHT process for material 14.60mm thick in a pressure vessel built to ASME section VIII division 2?   THE FIRST CHOICE IN TANK CONTAINERS DAVID STEVENSON TECHNICAL MANAGER Eurotainer U.S. INC. 5810 Wilson Rd. Suite 200, Humble, Texas, 77396 USA Phone 01 832 300 5019 (Direct)● Mobile 01 713 805 0192 ● Fax 01 832 300 5050 email: dstevenson@usa.eurotainer.com ● website: www.eurotainer.com  Please consider the environment before printing this document  

Re: [MW:12562] Carbides Precipitates on HAZ ; 625 Overlay on AISI 4130

Dear Sir,               I think u may have to use a buttering layer. 2011/9/27 K.Babu < kbabupsg@gmail.com > Gents, Do you have idea on the Inconel 625 Overlay on the AISI 4130/4140 I used P-GTAW, with 150deg cel as preheat & Max . Inter pass is 240 deg cel, PWHT -590 deg. Cel for 3 hrs to reduce the hardness to below 250 VHN In micro analysis, HAZ showing the carbide precipitates. Any idea, on why happened like this? Regards   K.Babu   -- To post to this group, send email to materials-welding@googlegroups.com To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com For more options, visit this group's bolg at http://materials-welding.blogspot.com/ The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents. -- regards, Harish. -- To post to this group, send email to...

RE: [MW:12557] Uncontrolled heating and cooling effect of Carbon steel below lower critical temperature

Limesh   Simple rule :  you will have no phase changes unless the steel is heated above the lower critical temperature (LCT).    If you have an alloy steel, the lower critical temperature will be different than for a carbon steel, but the above rule applies.   If the maximum temperature is below the lower critical, there will be no phase change but coarsening of pearlite will occur.  Other structural changes may occur but the phases will not be effected (creation of tempered martensite or bainite, redistribution of stresses, creep due to stress relief etc.).    The major reason heating and cooling rates are restricted are to prevent the creation of residual stresses usually caused by uneven distribution of heating/heat removal .  These stresses can cause cracking, particularly in highly restrained structures.   {Note with regard to the simple rule above,  there will be an apparent upward shift in LCT with increasing heating rate (d...

Re: [MW:12560] PWHT Requirement for SA 335 P91 (or P no. 5B Group 2/ 15E group 1)

@Raghuram ... Thank you very much for your prompt and sufficient response @Goswami Sir! Please see the table below. If you require more information i will forward  Regards ASIF +971-50-9198730 On Tue, Sep 27, 2011 at 4:00 PM, pgoswami < pgoswami@quickclic.net > wrote: Hello Asif,   I have seen the use of P-91 material in conventional thermal generation units, coal, HRSG ,Coal+Biomass. If the plant in question is a solar power plant, then what're the design and operating conditions (e.g temperature, pressure )?   Appreciate your response.    Thanks.   Pradip Goswami,P.Eng.IWE Welding & Metallurgical Specialist & Consultant Ontario,Canada. Email-pgoswami@ sympatico.ca , pgoswami@quickclic.net   From: materials-welding@googlegroups.com [mailto: materials-welding@googlegroups.com ] On Behalf Of Bathula Raghuram (Mumbai - PIPING) Sent: Tuesday, September 27, 2011 1:30 AM To: ' materials-welding@googlegroups.com ' Subject: RE:...