Skip to main content

Re: [MW:36054] Weld overlay on F6 Nm

1. Use Preheat of 150degC to 250degC. Higher preheat temperature may result in retained Austenite and also upon overlay cool it to Room temperature or temperature below the Mf (Martensite finish temperature).
2. Use ER/ENiCrMo3 for the barrier layer as well as remaining passes.
3. Perform PWHT at least 30degC below the Material tempering temperature to avoid softening due to coarsening of carbides or pearlite spherodization.
4. Post heat at 300degC after welding may be beneficial to drive away Hydrogen.

Thanks & Regards

J.Gerald Jayakumar

0091-8838619635



On Tuesday, 12 May 2026 at 05:12:45 pm IST, 'manish kulkarni' via Materials & Welding <materials-welding@googlegroups.com> wrote:


We are qualifying PQrs for 625 WO on F6 Nm.   I foresee risk due to micro structure changes due to higher PWHt temp against tempering temp of C6 Nm . 
Also checking hardness control for cracking in HAZ as service is very high sour and high pressure. 
So if anybody has qualified PQR , was checking on above parameters. 
Thanks , 




On Tuesday, May 12, 2026, 12:37 PM, sridhar cn <sridharcn305@gmail.com> wrote:

What problems are you expecting to face during pre and post overlay welding operations? 
You have not yet spelled out whether it will be Stellite, Ni based or SS based overlay and
on what thickness? 
Could mention only the expected problems and precautions /solutions to avoid them in advance. 
Unless the actual welding (PQR) is done, we will not know what practical problems to face. 
Think you can guide us with your experience.
All the Best!!
rgds,

On Mon, 11 May 2026 at 22:32, 'manish kulkarni' via Materials & Welding <materials-welding@googlegroups.com> wrote:
Yes, literature is available, but looking for actual production experience as normally martensitic SS.  , weld overlay is not performed. 
Regards,



On Monday, May 11, 2026, 4:04 PM, sridhar cn <sridharcn305@gmail.com> wrote:

 Though I have not done actual overlay, what I could gather from the available literature is that, F6NM Stainless Steel weld overlay is 

 commonly  done in hydro turbine parts, valve internals, and pump sleeves . The success of overlay depends much more on dilution control, 

 hydrogen control, and post-weld hardness management than on the actual deposition process itself.

 F6NM / CA6NM is a P6, air hardening low carbon martensitic stainless steel with approx. 13% Cr + 4% Ni + 1% Mo. Its UTS is 750-950 MPa,                                   Yield  550-750 MPa, 15-22% EL and hardness 259-320 HB. Major issues observed during overlay are: Underbead cracking; delayed hydrogen 

cracking; toe cracking after 24–72 hrs; hard martensitic HAZ overlay disbonding during service.This happens because F6NM transforms to 

untempered martensite very easily during cooling.Typical HAZ hardness without proper control would be 420–550 HV and highly crack-sensitive.

To avoid them, a  mandatory preheat at 150–250°C and an inter pass temperature of 180–250°C to be maintained. Low heat input should be  

avoided as  it causes fast cooling and forms martensite structure. Typical heat input range could be 1.5-2.0 kJ/mm. Excessive high heat input 

may create Ferrite in-balance. Final overlay (Stellite, Ni alloy 625 or SS)  should be done after buttering with ER 309L  to avoid martensitic cracking;  

PWHT at 580–620°C (furnace cooled up to 300 Deg C) for 2–4 hrs or controlled welding with preheat + slow cooling is recommended to improve 

toughness. Usually a 2- layer minimum deposit is done; First layer may have high dilution and the second or third layer will have required chemistry.

Low hydrogen consumables, dry shielding gas, and clean surface are required to avoid Hydrogen (due to moisture/contamination) are mandatory. 

Preferred furnace cooling or insulation blanket cover to avoid fast cooling. Recommended hardness targets are HAZ < 350 HV; Overlay transition 

< 380 HV; Higher values usually indicate cracking risk.

For restrained and heavy F6NM components, no direct deposit on the cold base metal should be done. Never stop welding midway and leave partially   

heated components overnight. Maintain minimum holding temperature until welding completion.  A large number of failures originate from thermal 

cycling interruptions.

Trust above info. may be of help to you. 

C Sridhar.

----------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------


On Fri, 8 May 2026 at 22:14, 'manish kulkarni' via Materials & Welding <materials-welding@googlegroups.com> wrote:
Hi respected group members,

Pl share some experience on weld overlay on F6Nm material?
Regards, 



On Friday, May 8, 2026, 7:15 PM, sridhar cn <sridharcn305@gmail.com> wrote:

From the available Technical literatures.
CS.

On Fri, 8 May 2026 at 09:58, Kannayeram Gnanapandithan <kgpandithan@gmail.com> wrote:
could pl  share the reference where it is given
THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015, ISO 3834, EN 1090 & EN 15085, 
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349


On Mon, May 4, 2026 at 3:18 PM Ashishranjan - Domech Fabricators Pvt.Ltd. <planningdfplril@gmail.com> wrote:
Yes, you can use multiple PQRs to support a single WPS under AWS as well but it’s handled a bit differently than in ASME Section IX, and you need to be careful about how you justify it.
  

Regards,

Ashish Ranjan

+91 9555864374

Go green logo

Save a tree...Please consider your environmental responsibility. Before printing this e-mail message, ask yourself whether you really need a hardcopy.



"Confidentiality Warning: This message and any attachments are intended only for the use of the intended recipient(s), are confidential and may be privileged. If you are not the intended recipient, you are hereby notified that any review, re-transmission, conversion to hard copy, copying, circulation or other use of this message and any attachments is strictly prohibited. If you are not the intended recipient, please notify the sender immediately by return email and delete this message and any attachments from your system.

Virus Warning: Although the company has taken reasonable precautions to ensure no viruses are present in this email. The company cannot accept responsibility for any loss or damage arising from the use of this email or attachment."


Caution: The e-mail below is from an external source. Please do not open attachments or click links unless this email comes from a known sender and you know the content is safe.



On Mon, Mar 2, 2026 at 2:56 PM praba karan <prabakaran776@gmail.com> wrote:
Dear experts,

For procedure qualification as per ASME SEC IX- "Multiple PQRs may support one WPS",

Likewise can we follow the same practice in AWS also?  Because which is not mentioned directly on the code that we can use multiple PQRs to support one WPS.(And I'm not using prequalified WPS)


Thanks & regards
Prabaharan

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/f0bb15a1-0ff5-4d62-b662-1b365472aadbn%40googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CA%2BRvhZDh_6WgTgTWMSGZ3qH0f9c_zMVttqjGZAyNV5MfzvFWgQ%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAJzm4eOijhd0u6mpPJa1bWXPukQzriRq%2B%3DBT09HmVumWdc9rBA%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAHo%3DYigufeqoyvHVLTFVMBp9%2BGGs8%3DwALx0OAe0FqSpTNCQ%2BMw%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1971004341.4329738.1778258131209%40mail.yahoo.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAHo%3DYijqD-%3DGL-6%2B%3DTCCSExVfU4S45RW%3D7t4_zBLgEJqgOmJZw%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1796566718.435064.1778517718084%40mail.yahoo.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAHo%3DYigjypi-QPe-Oag1ELByd4DJkpg%3DMvDFxrPTANoJeqjYjA%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/286676273.628607.1778583974674%40mail.yahoo.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...