Re: [MW:36032] Procedure qualification through AWS

Dear Mr Sridhar,

good & wishes for detailed explanation for welding of dissimilar material . All the inputs & parameters are found as good and meeting the standard requirements. small suggestion on PWHT temperature as given below:
as per ASME sec VIII div-1 for 410 type steel- PWHT temperature will be 760deg C, kindly check & proceed further       

Regards,
Sankaran.SP
Welding & Metallurgy expert
Coimbatore, India. 


On Tuesday, 17 March 2026 at 09:05:28 pm IST, sridhar cn <sridharcn305@gmail.com> wrote:


Giving below are the hints for WPS (both ISO / AWS) for joining SS 410 (martensite) to SS 316 (austenitic). 

This should be supported by a PQR qualification. 

WPS: Dissimilar Joint: SS 410 vs. SS 316 

1. General Information:

Process: GTAW (Root) + SMAW / GMAW (Fill & Cap); Type: Dissimilar stainless steel welding

2. Base Materials:

SS 410 (UNS S41000) – 410 Martensite SS to  SS 316 – Austenitic SS; ASME sec. IX P no 6 (410) to Pno 8 (316)

3. Joint Details:

Joint Type: Butt joint;  Thickness Range (Qualified): xx mm – xx mm (based on the PQR)

Root Gap: 2–3 mm; Bevel Angle: 60° included; Backing: Optional (SS backing or GTAW root) 

4. Filler Metal:

Primary Choice: ER309L / E309L (for welding);  Alternative (for critical service): ERNiCr-3 (Inconel 82)

GTAW: ER 309L / ER NiCr-3; SMAW: E 309L / ENiCrFe-3; GMAW: ER309L

(309L acts as a buffer to handle dilution & prevent cracking; Ni-base reduces risk of martensite cracking)

5. Welding Parameters: GTAW (root) Polarity: DCEN ; Shielding gas: Argon (99.99%) Flow rate: 10–15 L/min

SMAW (fill/cap).Polarity: DCEP; GMAW (Optional) Mode: Spray / Pulse; Gas: Ar + 2–5% CO₂ or Ar + 2% O₂ 

6.Preheat & Inter-pass Temperature: Preheat  200-300 degC (for SS 410 to avoid cracking); Inter-pass 250 deg.C. 

7. PWHT (for SS 410): SR at 650-700 deg C; Holding time- 1hr / 25 mm thick; Cooling- Controlled furnace cooling. 

8. Special Technique: Buttering recommended on SS 410 side with ER309L to void cracking; Stringer beads preferred (no weaving)

9. Inspection & Testing: 100% VT+ PT + RT / UT – As per the requirement;  Hardness check (important on 410 side & HAZ) 

Trust above details will help you to prepare your WPS & PQR.

 

Sridhar.

-------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------


On Tue, 17 Mar 2026 at 15:39, Md Usman Ghani <mdushmanghani@gmail.com> wrote:
Just for clarification
Can any one share, WPS, for ss410 to SS316,

On Mon, 2 Mar, 2026, 12:39 pm Sajeersayed Ali, <sajeersayed@gmail.com> wrote:
5.2.2 Combination of WPSs. A combination of qualified and prequalified WPSs may be used without qualification
of the combination, provided the limitation of essential variables applicable to each process is observed.


On Mon, Mar 2, 2026 at 12:26 PM praba karan <prabakaran776@gmail.com> wrote:
Dear experts,

For procedure qualification as per ASME SEC IX- "Multiple PQRs may support one WPS",

Likewise can we follow the same practice in AWS also?  Because which is not mentioned directly on the code that we can use multiple PQRs to support one WPS.(And I'm not using prequalified WPS)


Thanks & regards
Prabaharan

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/f0bb15a1-0ff5-4d62-b662-1b365472aadbn%40googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAOnS74cq4KK-zTQpm8Bf4F937_mA%2Biy1fSR0nLx7DBG1500NzQ%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAP4SqnW-G_NGyNhFN%3D2qU7E62ywLQhuqurnrYQz5JpQkKioviA%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAHo%3DYiinzjrFoZ%3DThPn68NByzU2%3DVyDkvOe%3DWVom-EOT41xKXQ%40mail.gmail.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...