Re: [MW:35283] SA335 P91 to SA106Gr.B Dissimilar Material Welding Procedure

Mr. Vijay,
Welding P91 to P1 requires careful consideration. due to differences in their thermal 
and mechanical properties. However you can try with:
a proper edge preparation and alignment (to avoid cracks during welding),
using E 9018-B9 /ER90S-B9 filler metals (GTAW is preferred) which are compatible,
preheat to 150-200deg. C throughout to reduce the risk of cracking during welding,
maintain an interpass temp. below 250 deg. C to minimise thermal stresses and 
avoid embrittlement of weld area.
maintain Argon purging throughout, use nominal current to avoid distortion & 
cracking in P91 material
PWHT at 730-800 deg C with proper holding and to relieve stresses,
allow controlled cooling to avoid embrittlement,
monitor for Carbon migration from P1 to P91 which will affect mechanical properties.

In a nutshell, careful adjustments in heat input, preheating & interpass temp. control, and 
PWHT are necessary to ensure a successful welding and maintaining structural integrity.
rgds,
Sridhar.






On Mon, 16 Sept 2024 at 13:07, Vijay Kumar <vijaytuty@gmail.com> wrote:
Dear Experts,

I need SA335 P91 to SA106Gr.B Dissimilar Material Welding Procedure with some reference codes. 

Please share 

Thanks 
Vijayakumar
+91 8238450968

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/be7e26e6-2446-4b69-8ed4-d10c5a074dcfn%40googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAHo%3DYiiLsz5%3Dqi-qf6-Z4j889xVeLXR_f%2BDGnN2SbGrs2rXtFA%40mail.gmail.com.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...