Skip to main content

Re: [MW:33007] Black soot in MIG

AC GTAW with water cooled torch & HF unit

Thanks & Regards may be suitable for sheet metal.

J.Gerald Jayakumar

0091-8838619635



On Thursday, 31 March, 2022, 04:16:04 pm IST, Prem Nautiyal <prem.nautiyal26@gmail.com> wrote:


Hi Anthony 

You may please try with 99.9995% Ultra Pure Argon gas. Use a gas cup size of 20#.

Use the forehand technique in MIG.
MIG always works with DC, for GTAW you should go with AC.

Use a better quality branded filler wire spool.

Regards 

Prem Nautiyal 
Welding & NDT Specialist 
Cell 9769316004

On Thu, 31 Mar 2022, 15:36 'james gerald' via Materials & Welding, <materials-welding@googlegroups.com> wrote:
Try AC current

Thanks & Regards

J.Gerald Jayakumar




On Thursday, 31 March, 2022, 01:03:59 pm IST, Anthony Dalisay <anthonydalisay6@gmail.com> wrote:


Dear experts,

We have been welding aluminized sheet using MIG welder with the following parameters:

Amps: 125
Volts: 29.5
TS: 50cm/min
Gas flow rate: 12L/min
Gas type : 18%CO2 and 82%Ar

However, I cant get rid of black soot (smoke) in the weld vicinity. What do you think, is the best way to do to achieve cleaner weld in aluminized sheet such as this? 

Refer to attached photo for reference.



Thanks in advance for your expert advice.

Regards,
Anthony
--
Anthony Dipasupil Dalisay
TWI AWeldI

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CALBzUBLiVBU2wnkd3MGhgAMdC%2BMzEjF4SXM%2BsdgMXQgp5MVh9Q%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/1137188882.137058.1648720763794%40mail.yahoo.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAEP2HKDay-8%2Be1ViPnRSb1--q7R5DGACFPVtccN7Fku7v9jA1A%40mail.gmail.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...