Dear Mr Pandithan,
In the machine I have selected the pulse mode itself. (GMAW-P). The position I am using is IG(rotating ) . As I am using the synergy mode in the machine the current and voltage is getting selected automatically when I am giving the wire feed speed. I am using the wire feed speed of 9.5 m/min, the voltage coming is in range 25V -28V and current in range 215 to 230. How to ensure I am not using the short circuiting mode?? I am using this process for pipe welding which includes both high and low thickness.
Regards,
Aby
On Wed, Mar 22, 2017 at 9:02 AM, Kannayeram Gnanapandithan <kgpandithan@gmail.com> wrote:
As argon increase, %of penetration will come down and may get into porosity . Try with 85+15 with current of >250amps. spatter is inevitable in this process, u can reduce by another option with GMAW-P. If u work in Spray mode, spatter stiking into base metal will be less due to its sizesTHANKS & BEST REGARDS,KG.PANDITHAN, IWE, AWS-CWI, CSWIP 3.1,CONSULTANT-WELDING & QUALITYMobile no: +919940739349On Tue, Mar 21, 2017 at 7:12 PM, Prasad Rao <prasadrao31@gmail.com> wrote:![]()
This message is eligible for Automatic Cleanup! (prasadrao31@gmail.com) Add cleanup rule | More info
Try for 98% argon and 2% co2--On Tue, Mar 21, 2017 at 12:56 PM, Aby Jose <abycscec@gmail.com> wrote:Dear all,--What shielding gas should be used for the pulsed GMAW welding of carbon steel? When trying with 80%Ar+20%CO2 mixture I am getting a lot of spatters. The welding used is Automatic welding with Robotic machine.Any recommendations???Regards,Aby
http://www.linkedin.com/groups/MaterialsWelding-122787?home= &gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com .
To post to this group, send email to materials-welding@googlegroups.com .
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CACdTRdy c8NMn6LBHHHTeYFxP_Ani0cnWDw0j5 qEJSyRyfoOe4Q%40mail.gmail.com .
For more options, visit https://groups.google.com/d/optout .
http://www.linkedin.com/groups/MaterialsWelding-122787?home= &gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com .
To post to this group, send email to materials-welding@googlegroups.com .
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAEML-XR .owcwexs%3DZz4xzozQA7Q6p6XcbJr1 YNpG98vBsr-o90w%40mail.gmail. com
For more options, visit https://groups.google.com/d/optout .
To view this discussion on the web visit https://groups.google.com/d/--
http://www.linkedin.com/groups/MaterialsWelding- 122787?home=&gid=122787&trk= anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com .
To post to this group, send email to materials-welding@googlegroups.com .msgid/materials-welding/ .CAJzm4eMRjCwxaG% 3DH62vgm57nrFmJuf8rLFrZX% 2BW9Tah%3D0wjHJg%40mail.gmail. com
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CACdTRdzxfYOOSzPmY0MZP09YPVeAXwyREZSr9%2B6GyYUGdL0%2BTg%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.
Comments