Hi
 
you can use metal wire ER70S-3 or you can use ER70S-2 provided that the lower impact test -48 
 
Regards
BOUDA superviseur QC TECHNIP   

Date: Mon, 23 Sep 2013 08:34:00 +0300
Subject: Re: [MW:18739] Which filler wire is suitable to achieve Impact Prop 20J at -48°C (P1 materials; GTAW)
From: m.a.samdani7@gmail.com
To: materials-welding@googlegroups.com

I used ER80S-Ni1 for SA-333 Gr.6 (P1-Group1).  I got  average 50 J (WM) and 72 J (HAZ) @ -40 c.


On Mon, Sep 23, 2013 at 8:00 AM, Saravanan Sornam <saravanshyla@gmail.com> wrote:
HI Ali Samdani ,

I have not used ER80S-Ni1 for P No.1 of such Low Tempr , because this filler comes under ASME II C , SFA 5.28 and also for Low alloy steels.

But for one of the PQR for Minus 47 Deg C especially for P No.1 , I have used ER70S-2, it gives Avg 60 J .

Please confirm again whether any preventive measures you have taken for using Low alloy welding consumable to weld P No.1.

Regards,
Saravanan,
Korea


On Mon, Sep 23, 2013 at 1:32 PM, Ali Samdani <m.a.samdani7@gmail.com> wrote:
For low temperature application, you may use ER80S-Ni1 for GTAW.


On Sun, Sep 22, 2013 at 11:50 AM, Mhaskar Aly <mhaskar.aly@gmail.com> wrote:
Dear Friends,
 
I have to qualify a PQR to achieve following properties, which filler wire is suitable.
 
PQR Data
·         Process GTAW
·         Material P1
·         PWHT 650° 180min
·         Impact Properties required 20J average at -48°C…
·         Hardness 200BHN max
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...