Re: [MW:18741] Which filler wire is suitable to achieve Impact Prop 20J at -48°C (P1 materials; GTAW)

You can use ER70S2 . But my question is you are mentioning P1 material and PWHT Time & Temperature you are showing is abnormal.
Generally for P1 you should go for 595 +/- 15 Degrees. The temperature you are showing is used for Low Alloy Materials P4 ...&
-  Time you are showing 180 minutes...means 3 Hrs...if you check UCS 56 of Section VIII Div 1 - 1 Hr per inch ...
-  You are mentioning only One process - GTAW... then what is your Test coupon thickness.
- Kindly check the Heat treatment Cycle before proceeding ..


Regards
Anil






On Sun, Sep 22, 2013 at 12:50 PM, Mhaskar Aly <mhaskar.aly@gmail.com> wrote:

Dear Friends,

 

I have to qualify a PQR to achieve following properties, which filler wire is suitable.

 

PQR Data

·         Process GTAW

·         Material P1

·         PWHT 650° 180min

·         Impact Properties required 20J average at -48°C…

·         Hardness 200BHN max

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...