Dear Friend,
 
If i am not wrong A336 Gr.6 such pipes are not avaliable, may that is A333 Gr.6 (LTCS), there are two methods for separations of this materail.
 
1. Perform Impact at -45° and whch passes the test is A333 Gr.6 and which fails is A106 Gr.B.
2. Perform chemical analysis by any method whcih can detect the following
     Ni, Cr, Co, Va, Mo, since A333 Gr. 6 does not have thease requirements whcih materail not having thease composition were     
     A333 Gr.6 materail.
 
Regards,
 
N.Nageswararao
    
On Sun, Feb 15, 2009 at 4:25 PM, tamma reddy <tsr_52@yahoo.co.in> wrote:
Dear Friends,
 
When A106 Gr.B and A336 Gr.6 pipes are physically mixed up and mill identification/ stencilling was lost during painting on external surface. Since both are CS materials, segregation by PMI (i.e by X-Ray spectrometer or by Gamma ray) is not possible.
 
Is there any other NDE method to segregate/ identify them to the respective material specification.
 
Regards,
T S Reddy



Add more friends to your messenger and enjoy! Invite them now. --~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...