[MW:991] Re: 975] RE: 968] SS431#SS 304L

 
Dear friends

The UNS number of SS 431 is UNS:S43100 ,( ASTM A473 type 431).
Now if we use E309L to Weld SS304L # SS 431, is any PWHT required?
Also if we use E410 electrodes then i think PWHT is required. We want to avoid PWHT in job. SO shall we use E309L SMAW electrodes for welding without PWHT. What do you say about preheating ?

Regards

Prem Nautiyal
Godrej,Vikhroli.

On Tue, 29 Jul 2008 Abby Joseph wrote :
>I presume you are referring to UNS No. S43100.
>
>Welding of this steel to 304L should be done with 309L consumables.
>
>
>
>Regards,
>
>
>
>Abby Joseph
>
>T-PUT Welding India Pvt. Ltd.
>
>
>
>
>
>  _____
>
> From: materials-welding@googlegroups.com
>[mailto:materials-welding@googlegroups.com] On Behalf Of Bathula Raghuram
>(Mumbai - PIPING)
>Sent: 28 July 2008 10:15
>To: materials-welding@googlegroups.com
>Subject: [MW:975] RE: 968] SS431#SS 304L
>
>
>
>Please specify UNS# for SS431?
>
>  _____
>
> From: materials-welding@googlegroups.com
>[mailto:materials-welding@googlegroups.com] On Behalf Of PREM SHANKARDUTT
>NAUTIYAL
>Sent: Friday, July 25, 2008 8:02 PM
>To: materials-welding@googlegroups.com
>Subject: [MW:968] SS431#SS 304L
>
>Dear Friends
>
>Has anybody welded SS431(martensitic Stainless Steel) to SS 304L?
>We have a SS431 forging about 50mm thick and it has to be welded to a 25mm
>thick SS304L ring. The joint is a 4mm fillet all around.
>Can anyone tell me the welding procedure, precautions and SMAW electrode to
>use. Can we use E309L electrode?
>
>Regards
>
>Prem Nautiyal
>Godrej,Mumbai
>
>PREM S NAUTIYAL
>CELL : 9820313278
>
>
>
>
>
>
>
>>

PREM S NAUTIYAL
CELL : 9820313278


--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...