Hi Kannayeram Gnanapandithan,

 

The soak temperature and time for a hydrogen bake-out, or dehydrogenation heat treatment (DHT), depends on the size (diameter) and thickness of the weld.

A temperature of only 50 to 100 degrees above preheat temperature, for a time of only 30 minutes, is generally inadequate to ensure 100 % removal of hydrogen.

Email us the diameter and thickness of your weldment assembly, and we will recommend the DHT soak temperature and time for 100 % removal of hydrogen.

 

Regards,

Dennis Thompson, P. E.

Manager, Technical Support Group (TSG)

Dennis.Thompson@TeamInc.com

 

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Kannayeram Gnanapandithan
Sent: Thursday, January 31, 2019 10:02 PM
To: materials-welding
Subject: Re: [MW:29021] Interpretation available (IX-04-03)

 

EXTERNAL EMAIL

 

50 to 100 degree above preheat temp. Holding time minimum 30minutes . As per ASME it is not essential variable but it is good Engineering practice for carbon steel above 40mm, 

 

On Fri, 1 Feb 2019 8:25 am bilal wahla <bilalwahla047@gmail.com wrote:

Dear Friend,

Purpose of post heat is to DIFFUSE hydrogen after welding , for this purpose we hold our joint at 93-80 degree for 1 hour after completion of welding.

PWHT always Performed below Lower Transformation Temperature, PWHT and Post Heat is different things.

Kind Regards 

 

 

On Tue, Jan 29, 2019 at 2:27 PM George Dilintas <dilintas@gmail.com> wrote:

Most propably your client wants you to perform a hydrogen bake-out treatment 

 

Στις Δευ, 7 Ιαν 2019, 08:58 ο χρήστης muneebslsa@gmail.com <muneebslsa@gmail.com> έγραψε:

Hi All,

Client specification calls for post weld baking/heating (not stated as PWHT) of a P No.1 material after welding for a specific reason. Does it consider a PWHT condition as per ASME Sec IX QW-407.1(a) Point#2, i.e PWHT below lower transformation temperature? If it is considered as PWHT as per the clause above, then would a PQR with 200 Deg C PWHT qualifies to perform PWHT on the weld at 600 Deg C which is below the lower transformation temperature of P No.1 keeping all other essential variables same. Note: Though there is an interpretation available (IX-04-03), it doesn't state the answer instead it refers to QW-407.1 (throwing the ball away wisely).



Originally posted in Linkedin



by



 


Regards,

Mohamed Muneeb Mahaboob

CSWIP 3.2-89247/2

IRCA-9001:2015 LA

ASNT-NDT-L2-RTFI-RT-UT-MT-PT.

SAP#:70021650 APs:JAPID, QCS & QCI.

muneebslsa@gmail.com M +91-636-955-7189

''If you know any art by any means then SCULPT IT - no matter how cheap or useless it is - JUST SCULPT IT, you will never know when experts will be on demand'' 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.


 

--

Respected Sir,

 

Please find the enclosed file.

 

Bilal Arshad Wahla

P.W.H.T Engineer

SEPCO Electric Power Construction Corporation

Saudi Aramco JAZAN IGCC Power Block Project (EPC-4)

Jazan Economic City, KSA 

Mobile: +966 591317207

Email: bilalwahla.047@gmail.com

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...