Monday, August 29, 2016

Re: [MW:25328] Hard Facing_Stellite 6 _reg

HI

Did you use any Buffer layer prior to ST6, if not use E312 XX type electrodes as a base layer .

use stringer bead

regards

DAS

On 28 August 2016 at 22:18, Sivaraman N <nsivaraman9@gmail.com> wrote:
Dear all,

While doing Hard facing Overlay of stellite 6  on carbon steel and stainless steel  cracks observed during second layer and third layer


Base Material:SA 516 Gr 70 (15 mm thk) & SA 240 TP 316 L(15 mm thk)
Electrode:ECoCrA
Process: SMAW
Overlay thickness:6 mm

How to avoid the cracks during hard facing?

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/8afcb0ec-7cc7-4414-be0c-f3a4d82b5f32%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJyLdkoxA6a52Yq4wgoEWPU7G-_UWM4Sy4Vi55TA1t51xf0U%3Dg%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...