Re: [MW:25276] Post Forming Heat Treatment of SS316L Dish

PFHT is not mandatory as per code.
Some client specify PFHT as solution annealing if hardness after forming is more than 22 HRC

PVG

On 21 Aug 2016 17:08, "A Ahmed Ahmed" <1aajtak1@gmail.com> wrote:
Dear All,

Code: ASME SEC VIII-1

Post forming Heat Treatment of Dish...

MOC: SS316L

Design Temp 85°C

Fibre Elongation: 3.6%

UHA-44 table does not show values of Fibre elongation..

Is PFHT required for this dish.

Kindly advise

Ahmed

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CA%2BL7tiPwcXf8BVFYiF_b%2BCF3jdfsjhVdQGAyK-FfvAhpWOZDOQ%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAEi5r3YaX6d%3D%2BpdHEZ_A6kh4Z4t6WB0MnwpT2KGKi2VGUuiGUQ%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...