Re: [MW:35740] ASME IX WPS Qualification Query: GTAW + FCAW with Multiple PQRs

Your first PQR covers GTAW + SMAW + SAW (with Impact + PWHT), your second PQR covers GMAW + FCAW with no indication of impact or 

PWHT. None of the PQRs individually or jointly cover the specific combination of GTAW + FCAW with impact + PWHT.

You cannot take GTAW (from a PQR qualified with SMAW/SAW) and FCAW (from a PQR qualified with GMAW), unless both cover impact/PWHT 

and are qualified for the intended sequence as in production.

ASME Section IX does not permit combining processes from unrelated PQRs to make a new process combination (e.g., GTAW from one PQR and 

FCAW from another, unless the conditions of QW-200.4 or QW-200.4(b) are strictly met—typically for root/fill passes.

QW-200.4 enables the use of multiple PQRs for one WPS but strictly constrains the qualified ranges and mandates that all code requirements be 

satisfied with the intended production.

You need to qualify a new PQR with GTAW + FCAW (Impact + PWHT) as performed for production.

The code does not use language that "explicitly prohibits" such combinations. Instead, it imposes conditions; the resulting WPS must not exceed the 

qualified ranges of thickness, essential variables, base materials, and other requirements demonstrated in the PQRs.

C Sridhar

-----------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------------


On Mon, 28 Jul 2025 at 08:03, Saurabh Jain <ensaurabh@gmail.com> wrote:
Dear Welding Experts,

I'm currently preparing a Welding Procedure Specification (WPS) and have encountered a request to qualify a GTAW + FCAW(IMPACT+PWHT) process combination by referencing two different Procedure Qualification Records (PQRs). The first PQR on hand covers GTAW + SMAW + SAW(Impact+PWHT) while the second covers GMAW + FCAW.


My concern is that combining these PQRs in this manner for a GTAW + FCAW WPS might not align with the requirements of ASME Boiler and Pressure Vessel Code, Section IX. 

I would appreciate clarification: Is it permissible under ASME Section IX to qualify a GTAW + FCAW WPS using these two separate PQRs? If not, which specific clause(s) in ASME Section IX address this limitation?

Regards 
Saurabh Jain

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CADr-LL9K%2B_fuWrPQQwajEpfBoYJmtvctid0VQ3SraZssRy%2BVdw%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAHo%3DYihY8cRrp-KomgECA99%3DJa9x87Csp1zkDkVZz7AkMF1A%3Dw%40mail.gmail.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...