Re: [MW:32356] filler material between 304L and 316L

You can use either ER316L or ER308L welding consumable.

below from API 582

Inline image


AWS D 1.6 recommends 308L as below.


Inline image

Technically the Base metal dissimilar (304L & 316L) will be subjected to the same process fluid as the weld metal lower or higher side.



Thanks & Regards

J.Gerald Jayakumar



On Saturday, 8 May, 2021, 09:45:21 am IST, Chiranjeevi A <chiranjeevipuvvula@gmail.com> wrote:


Dear Experts,

     At the site 308L filler wire used for the Pipe joint between 304L and 316L.  After doing the PMI QC rejected the joints and suggesting to use 316 filler.

   Experts kindly share the details of the code reference to accept or any procedure to avoid cutting 20joints.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAN4%2Bm0xA0VB5ScFArEbYRJMODF7D%2B0dwsfdrL4qO1GygpVXhzg%40mail.gmail.com.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...