Thursday, April 17, 2014

Re: [MW:20614] RE: 20584] Quarry regarding SFA 5.5

Dear Mr. Nikdin:

The reason why Ni+Mn should not exceed 1.5% is that it lowers the AC1 (austenitization temperature) which will cause either of following complications:

  1. Either your AC1 comes down and it is possible that PWHT temp goes higher than AC1, then instead of stress relieving you will see martensite formation during cooling which increases your hardness and creates new residual stress.
  2. Or you know about the above problem and are going to be careful about passing AC1. But your PWHT temp will drop below the required temperature for stress relieving. It means that either you do not relieve the stress or it will take a long time and costs you a lot.
Hence, it's better to limit the Ni+Mn content and save the trouble.

 

Best Regards

Ramin Kondori

Sr. QA/QC engineer

Yadavaran Oilfield Project

SIPC (SINOPEC)



On Mon, Apr 14, 2014 at 7:07 PM, John Henning <jhenning@deltak.com> wrote:

Ni and Mn depress the lower transformation temperature and the martensite finish temperature.  If excessive can result in PWHT being intercritical and/or the weld having retained (untransformed) austenite. 

 

John A. Henning

Welding & Materials

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Himan Nikdin
Sent: Sunday, April 13, 2014 11:22 PM
To: materials-welding@googlegroups.com
Subject: [MW:20584] Quarry regarding SFA 5.5

 

Dear Experts

 

As per note "J" of Table 2 of SFA A5.5 (SPECIFICATION FOR LOW- ALLOY STEEL ELECTRODES FOR SHIELDED METAL ARC WELDING) which contain chemical composition requirements for weld metal Ni+Mn content shall be max. 1.5% for E9015-B9, E9016-B9, E9018-B9, the question is why?

 

Regards,

Himan Nikdin 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.


______________________________________________________________________
The information in this email is confidential, and is intended solely for the addressee(s). If you are not the intended recipient of this email please let us know by reply and then delete it from your system; you should not copy this message or disclose its contents to anyone. The internet can not guarantee the integrity of this message. HAMON (and its subsidiaries) shall (will) not therefore be liable for the message if modified.
______________________________________________________________________

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...