Re: [MW:20612] Material hardness of 514 GR F

Dear Tahir:

Use low heat input welding processes. The lower, the better...
GMAW-Spray mode is good but pulsed arc works magic for these Q&T materials.
Do not forget to control so that you do not exceed preheat and inter-pass temp ranges.

 

Best Regards

Ramin Kondori

Sr. QA/QC engineer

Yadavaran Oilfield Project

SIPC (SINOPEC)




On Wed, Apr 16, 2014 at 1:59 PM, tahir alam <tahiralam007@gmail.com> wrote:
Dear Experts

we try to qualify PQR of Material 16 mm 514 Gr F in 2G and 3G position.we did the testing of tensile test ,bend and hardness test.Tensile test and bending test is satisfactory but vickers hardness number is more in HAZ(i.e 322) .Here while doing welding of piece we maintain the preheat temperature of 400F and interpass temp of 200F.But according to client hardness should be 250 max.Can u advice me how to reduce the hadness in HAZ while doing welding of test piece.

Kindly advice me any method to maintain hardness 250.

Best Regards
Tahir Alam
Planning Engineer
Agam Tank Maintenance Group
Mobile : +(965)5150-1509


--------------------------------------------------------------------------------
Site Office : +(965)2388-3614
Head Office : +(965) 2398-5381l2
Fax : +(965) 2398-8312
P.O.Box : 9390 Ahmadi, 61004 Kuwait
Email : tahiralam007@gmail.com
Website : www.agamltd.com
-------------------------------------------------------------

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...