[MW:803] Re: Dissimilar Group number/Thickness combination PQR as per QW403.5/QW403.6

 
QW 202.4 allows you weld dissimilar thickness material in Production with a qualified PQR(s). Not for the qualification of dissimilar thickness. The thickness Qualification range is to be taken from QW 451or QW 403.6 (if impact test is required) from the thickness used for qualification.
For qualification you need similar thickness (for full penetration groove welds). You can use dissimilar thickness but you will not get the benefit from thicker material (thickness) as the thickness T considered is based upon the tensile specimen thickness used.
Please refer Section IX Interpretation No. IX 86-43 which is nearly similar to this query.
Thanks & Regards,
Sanjeevan
 
----- Original Message -----
From: "Bathula Raghuram (Mumbai - PIPING)" <R.Bathula@ticb.com>
Sent: Tuesday, May 27, 2008 9:06 AM
Subject: [MW:798] Re: Dissimilar Group number/Thickness combination PQR as per QW403.5/QW403.6


Min qualified thickness can't be 1.5mm, when impact testing required.
Qualified thk range for P1G1 will be 6-12mm and P1G2 would be 12-24mm,
please refer the question again.

Dissimilar thickness combinations are quite common to qualify (in
particular for SR nozzle welds on equipment) per QW202.4

-----Original Message-----
From: Quality [mailto:quality@gpsoman.com]
Sent: Tuesday, May 27, 2008 10:28 AM
To:
materials-welding@googlegroups.com
Subject: Re: [MW:797] Re: Dissimilar Group number/Thickness combination
PQR as per QW403.5/QW403.6


The qualified thickness range is 1.5mm to 12mm (2T) for P1G1to them
selves,
P1G2 to themselves & P1G1 to P1G2 combinations.

The maximum qualified weld deposit is 2t (to is deposited weld thickness

during the qualification).

If you qualify a procedure with different parent material thickness
(groove
weld), the thickness T can be considered based upon the tensile specimen

thickness (T) used for the destructive testing of the groove weld PQR.
In
short, qualification of different thickness of relatively less use in
ASME
Sec IX.

Normally none of the construction/ fabrication codes does not allow
difference in thickness more than 1.5T (of the thinnest). Any Thickness
welded above 1.5 will not be accounted in design.

Regards,
Sanjeevan
GPS

--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...