Skip to main content

200 series Vs. 300 series stainless steels

QUESTION:
High metal prices, especially for nickel and molybdenum, have our procurement people looking at less expensive stainless steels like the 200 series. Are these as good as 304 and 316 stainless steels?

ANSWER:
Before answering this question, let’s look at the history and differences between the 200 and 300 series stainless steels. The original 200 series stainless steels were first developed in the 1930s by using manganese to replace some of the nickel in the 300 series austenitic stainless steels. Certain elements used in stainless steels either promote the formation of the austenitic or ferritic atomic structure, and the austenitic stainless steels are the more corrosion resistant. The austenitic-forming elements are nickel, manganese, nitrogen, copper and carbon. The primary ferrite-forming element is chromium.

Since a stainless steel needs 10-12% minimum chromium to be considered “stainless,” it then takes about 8-10% nickel to offset the ferritic-forming tendency of chromium to make a stainless-steel austenitic more corrosion resistant. Historically, manganese has always been a lower cost element than nickel. So whenever there is a scarcity of nickel (as there was in the 1970s) or when nickel prices are high, such as they are now, people look to the 200 series stainless steels as lower cost alternatives.

But before deciding to use a 200 series stainless steel, there are issues to be considered. To further complicate the matter, there has been an increase in newer chrome-manganese grades developed and produced in Southeast Asia and China. The 200 series now represent 34% of China’s production of stainless steels.

Facts About the 200 Series

There are two categories of the 200 series stainless steels—those that only replace some of the nickel with manganese, such as the original 201 or 202 grades, and those that replace most of the nickel, such as the newer grades now being seen in Asia. These newer low-nickel grades also tend to have lower chromium, which further decreases their corrosion resistance.

To date there are no international standards for the use of these newer grades. To add additional confusion, users of stainless equipment, such as valves, know that magnetism—or more correctly, the lack of magnetism—is a way of verifying they have received the superior 300 series stainless steels. Since 200 series grades are non-magnetic, this could cause a buyer to mistakenly believe they have the correct and more corrosion-resistant 300 series stainless steel. In fact, there have been a few instances of deliberate mislabeling of 200 series grades as being 304 stainless. Some scrap dealers also still rely on magnetism to sort the 300 series grades from the magnetic and less corrosion-resistant 400 series stainless steels. Thus, the proliferation of the non-magnetic 200 series grades could lead to some serious scrap contamination issues if recyclers are not careful.

The first indication as to whether these grades are equivalent to 304 and 316 is they receive little attention until nickel either becomes scarce or when nickel prices are high. The primary reason they do not see greater use is simply because they are not as corrosion resistant as 304 and 316 stainless steels. However, the 200 series grades do have several beneficial uses, including cookware, railcars, lighting columns, washing machines and most mildly corrosive applications.

Problems with Corrosion

While the 200 series alloys do have good atmospheric corrosion resistance, they do not have good resistance to most corrosive chemicals. In addition, because most of the 200 series alloys tend to have a higher carbon content to help promote the austenitic structure, it makes them more susceptible to intergranular corrosion. Other characteristics that make the 200 series less attractive include their tendency to be more work hardenable and their potential to have slightly inferior surface finish.

So if you really need to lower your cost, you need to be very careful in the application of these 200 series stainless steels. A better choice would be to look at some of the duplex stainless steels such as S31803. The duplexes have about half the nickel of the 300 series so at the higher nickel prices they may be less expensive than the 300 series while providing comparable corrosion resistance. There are also some new lean (lower nickel) duplex grades on the market that may be even more cost effective. In any case, be sure to deal with reputable and knowledgeable suppliers who can assist you with the proper material selection.

Thomas Spence is director of materials engineering of Flowserve Corporation (www.flowserve.com). Reach him at TSpence@flowserve.com. The author wishes to acknowledge the assistance of Don Bush, materials engineer, Emerson Process Management-Fisher Division (www.emersonprocess.com).

Source: Valve Magazine

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...