Dear Karthick,

Have you asked for a consumable with heat treatment condition..? Check your certificate if is 3.1? Have you tried other hardness methods?? 

On Wed, Jul 10, 2019, 1:41 PM Karthikeyan Muthuvel <m.karthick2020@gmail.com> wrote:
Dear Experts,


Good day.


We had used the consumables (ER70S-2) / OK TIG ROD 12.62, Size : 2.4mm Dia. for our Production weld joints (Pipe materials : Carbon Steel ASTM A 106 Gr. B; Size : 3" X Sch 40). further to inform you that we had checked the Hardness of Base material , HAZ & on weld Metal before & after PWHT (below hardness readings were observed).


HARDNESS VALUES BEFORE PWHT

  1. Base material : 130 to 150 HB
  2. Heat Affected Zone : 140 to 160 HB
  3. Weld Metal : 170 to 190 HB


HARDNESS VALUES AFTER PWHT 

  1. Base material : 120 to 140 HB
  2. Heat Affected Zone : 130 to 150 HB
  3. Weld Metal : 210 to 250 HB


After performing PWHT the hardness value of Base material & Heat Affected Zone has been reduced. whereas the Hardness value of Weld Deposition has been increased (which is beyond the acceptable limit). 


So, I would like to know from you that what might be the technical reason/root cause for increase in hardness only on the weld joint after PWHT. 


Below are the PWHT parameters fyi.

Soaking Temp. : 620 Deg C

Soaking Time : 1 hr.

Rate of Heating : 100 Deg C per Hour (from 100 Deg C)

Rate of Cooling : 100 Deg C per Hour (Upto 100 Deg C)


Note:

  1. We had performed nearly 30Nos. of Production joints & we had face the problem of Hardness on all the weld joints. 
  2. Hardness was tested using Mic 10 tester method ( even cross verified with Equotip method & Tele brinell Method)


Thank you for your support.


Warm Regards,

KARTHIKEYAN  M.
QA/QC Inspector
Saudiarabia
Mobile:+966-501176985,
P Save A Tree - Please do not print unless really need

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAL7K%3D_LYvWPf_Tv3dhbLD9QfVUeJGvCGFLD4kLDtw3h9%3DF4W-A%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAKT-TupmJav6H1mShjX5HJEgDaCMs43VRTEkLgYeKgOkFgW-4w%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...