Sunday, July 14, 2019

RE: [BULK]Re: [MW:29830] HIGH HARDNESS AFTER PWHT (ER70S-2)

Hi,

 

Please see the suggested composition of ER-70S2 filler as per ASME Sec-II, Pt-C. The highlighted elements (Ni, Cr, Mo) may cause excessive hardness, together with presence of higher "C". Note the single value of "C" is the maximum. You need to check the consumable TC. Perform a ASME Sec II, Pt-C, bead on deposition test (with PWHT) to check the hardness.

Unless , project specifications calls for a restriction of hardness and if the PQR meets the other mechanical testing requirements , it should be accepted as per Sec-IX.

 

Thanks.

 

P.Goswami.P.Eng, IWE.

Independent Welding & Metallurgical Specialist

Linkedin: https://www.linkedin.com/in/pradip-goswami-2999855/

Email:pgoswami@quickclic.net,pradip.goswami@gmail.com

Cell/Whasapp:1-905-9793232

 

 

 

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Lu, Feng
Sent: July 12, 2019 8:56 AM
To: materials-welding@googlegroups.com
Subject: RE: [BULK]Re: [MW:29824] HIGH HARDNESS AFTER PWHT (ER70S-2)

 

Try to weld with 98%Ar – 2% O2.  The addition of Oxygen will remove residue Zr and Ti which are both strong carbide formers.

 

Do hardness measurement before and after PWHT to see if hardness still increase after PWHT.

 

 

Feng Lu, Ph.D., NDE Level III
Metallurgy and Welding Engineer

Zachry Industrial, Inc.
3600 West Sam Houston Pkwy South

Suite 200

Houston, TX 77042

luf@zachrygroup.com
Office: 713.979.2648
Cell: 512 797 5777
www.ZachryGroup.com

This e-mail may contain confidential and privileged material for the sole use of the intended recipient. Any review, use, distribution or disclosure by others is strictly prohibited. If you are not the intended recipient (or authorized to receive for the recipient), please contact the sender by reply e-mail and delete all copies of this message.

 

 

 

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Eyup Tan
Sent: Friday, July 12, 2019 1:30 AM
To: materials-welding@googlegroups.com
Subject: [BULK]Re: [MW:29822] HIGH HARDNESS AFTER PWHT (ER70S-2)

 

Check pipe materials may be different with certificate

iPhone'umdan gönderildi


Ramin Kondori <raminkondori@gmail.com> şunları yazdı (12 Tem 2019 07:22):

Please remember that without PWHT, you do not see any changes in the hardness. 

When you see an increase after heat treatment, most of the time these elements are responsible.


Ramin  Kondori

Sr. QA/QC & Welding Engineer

-----------------------------------------------------------

PG-Dip. in Welding Engineering (IWE  AT  0070)

BSc. in Civil Engineering (IUT)

BGAS Painting Inspector

ASNT Level I&II

                        

IIW-Logo-Colour-small

 

 

On Fri, Jul 12, 2019 at 8:49 AM Ramin Kondori <raminkondori@gmail.com> wrote:

It should be available online.

But to fully understand it I recommend the following:

 

First, if you should check the filler metal certificate or specification, you can easily spot these elements in chemical analysis requirement and report.

Then you can search for the articles about the effects of these elements on mechanical properties (especially hardness) of the steel, especially after heat treatment. These elements have some kind of secondary hardening effect on steel which is only appreciable after tempering. On the other side, PWHT is usually in the same temperature range as the tempering heat treatment operates. Therefore, you should expect the same effects & results which include an increase in hardness. 

 

To have a better idea on this subject, just look for the heat treatment methods for increasing strength and hardness. Many of them include adding these elements to the alloy and then subjecting the steel to a QT or NT heat treatment. You will see the connection.

 

Regards

Ramin  Kondori

Sr. QA/QC & Welding Engineer

-----------------------------------------------------------

PG-Dip. in Welding Engineering (IWE  AT  0070)

BSc. in Civil Engineering (IUT)

BGAS Painting Inspector

ASNT Level I&II

                        

IIW-Logo-Colour-small

 

 

On Fri, Jul 12, 2019 at 7:52 AM Raghuram Bathula <raghurambathula@gmail.com> wrote:

Intersting Mr Kondori

Do you have any refernace or research paper on this subject?

 

Thanks

 

On Thu, 11 Jul 2019 at 09:23, Ramin Kondori <raminkondori@gmail.com> wrote:

Hello,

 

ER 70S-2 is a triple deoxidized steel welding wire. 

It has Ti, Zr, and Al additions (please check your filler metal certificate).

After PWHT, these elements can increase the hardness of weld metal (but not HAZ or base metal). Many do not consider this when choosing filler metal.

 

I recommend you to conduct a chemical analysis examination on both the filler metal (rod or electrode) and production weld metal and revert back to us. 

 

Regards

Ramin  Kondori

Sr. QA/QC & Welding Engineer

-----------------------------------------------------------

PG-Dip. in Welding Engineering (IWE  AT  0070)

BSc. in Civil Engineering (IUT)

BGAS Painting Inspector

ASNT Level I&II

                        

IIW-Logo-Colour-small

 

 

On Wed, Jul 10, 2019 at 2:11 PM Karthikeyan Muthuvel <m.karthick2020@gmail.com> wrote:

Dear Experts,

 

Good day.

 

We had used the consumables (ER70S-2) / OK TIG ROD 12.62, Size : 2.4mm Dia. for our Production weld joints (Pipe materials : Carbon Steel ASTM A 106 Gr. B; Size : 3" X Sch 40). further to inform you that we had checked the Hardness of Base material , HAZ & on weld Metal before & after PWHT (below hardness readings were observed).

 

HARDNESS VALUES BEFORE PWHT

  1. Base material : 130 to 150 HB
  2. Heat Affected Zone : 140 to 160 HB
  3. Weld Metal : 170 to 190 HB

 

HARDNESS VALUES AFTER PWHT 

  1. Base material : 120 to 140 HB
  2. Heat Affected Zone : 130 to 150 HB
  3. Weld Metal : 210 to 250 HB

 

After performing PWHT the hardness value of Base material & Heat Affected Zone has been reduced. whereas the Hardness value of Weld Deposition has been increased (which is beyond the acceptable limit). 

 

So, I would like to know from you that what might be the technical reason/root cause for increase in hardness only on the weld joint after PWHT. 

 

Below are the PWHT parameters fyi.

Soaking Temp. : 620 Deg C

Soaking Time : 1 hr.

Rate of Heating : 100 Deg C per Hour (from 100 Deg C)

Rate of Cooling : 100 Deg C per Hour (Upto 100 Deg C)

 

Note:

  1. We had performed nearly 30Nos. of Production joints & we had face the problem of Hardness on all the weld joints. 
  2. Hardness was tested using Mic 10 tester method ( even cross verified with Equotip method & Tele brinell Method)

 

Thank you for your support.

 

 

--
https://secure-web.cisco.com/10-Q7BscgIuZcDyxU2XAmQaz3dg1kEbY50sAPyctI9NZ3DPQWGvuCGuHr50kuytAWzWxl-hOkXF-KpaGZCP01WLWinkIYQsfbSn_TCBq9eBhavMXgvKrh8U8wl_mKhf6cjtcQqYr1SWMndzkJxuVucwy0cheFkvk6I7XogL5O794izbwfrdR5_Zud68IA-o4sG4GDt4ebSeFj3TNUx6CJYpZwbVmLOCj7p4V_3vuatXBICrjFRaGbdhxPoirHcPz8Ig5DCkSCAMNZStgWr5vsQ0lM9r0rYPKkWnniWzPsbfkTiyiNo-dd5C1azWW2XVu2Z87rjuan4gXx6vhGTvoKWWPErw7KsfPcsv7wqAVH7qY/https%3A%2F%2Fmaterials-welding.blogspot.com%2F
https://secure-web.cisco.com/1LaBBAILJYgmsbnSiKOfNp4ERvxsTdASCAhfAjU3ytDGUYfkr4LT3rCBhTOd9EFLxAIdkwUK8Fkv2JvoEDXqazVSCNlnQj8CdjCU-P82n0uIx7JF2Tsg50IWDNaIkVtsnRWa3pjWZPX6_80IL5rtOnwFZWznAPMd0pasP5sR6goNTJqmQ9ZW5zk5ByYRfNMlluKhP_apveHS2-75mgnbf5_FdO07-rbh5JfMllO-Yiq1dBogPBjSXY0Jw5J1I0Y-_LhuKEdoPGk_WvCtqTY2N14HdbfSII3bhrvjiDNr8Ex63dJmnnB6cH-1O28dws9dBoBi8IC5ooGJfskiretOCkemXLaEBBVKj85cnUf_Jkkc/https%3A%2F%2Fwww.linkedin.com%2Fgroups%2F122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://secure-web.cisco.com/1lAkJPqs7ChEoKdMghq2xCdj16PWJE72RRsw-SXhGHlXXGB9Prd5n7ZubsClw7pm85MGpPdll3-SV656b4j8PV6O-26yogjXLkeu6qgg5H1A57dy91IE6XOHysalcdeljtfnL9grWZiQZeewqG0A5MWJQm_e2it65AkxnyhALPCGJFGo2u-G5cQNDmofoIC4ixLjTIBAjWi7cG2FfyTHOZ-d1gwzAWi0DNewtJNEipQ0oUo_HE5h1xpj0uFuj4Q1gpmyPpeEVyQug4d6a9B6gXC7V0SUjIeT8eJ80KVn4dzIIGudDSmGE-qAuFu3BBQqmp7AT4eL7D-64l9QJvW6h1jv_NGrCw3fro0k-MP90g4k/https%3A%2F%2Fgroups.google.com%2Fgroup%2Fmaterials-welding.
To view this discussion on the web visit https://secure-web.cisco.com/1x4FK-qaw25RErcFOKnYbRgs5sZXrtYuhy_To3vbKl2nmOUYF5iM4cG6yJiafg-3m28VOMWQdEVPal0Frqr5d7HpEi-TrRg65ybYHadgPaxMyu33w-fWrk5rJR0WmHipdo1EmAg34yzrIkZBKQKnbes7SVP_DI7p_d35CvG24JHZz1-o73kMI2qvb_149UO6uItEQn1eTwu4oxFdZIxwqyRU-AkGOSvSLPax2w0TsDUfwuneUDviLCLe-g-LCPDwT8yLQsw87Jmv8TAEZuId6tYOB98Pow76diWh35sMIyc6535fhUd2rbW9xAc1ycsY7AgJcitJ4uilzRBm8DwpyY_4LqQ61hdrW9yYICI0nzb0/https%3A%2F%2Fgroups.google.com%2Fd%2Fmsgid%2Fmaterials-welding%2FCADxVubnMbVdbBKU-tm69PK5ZZD%252BE1kq5KW4gFtgoWp%252B6TvOYsA%2540mail.gmail.com.
For more options, visit https://secure-web.cisco.com/17ZDQAS8Qh0iUezgzDaXyOBC-ym4sireR_UaTz9PS0LTp88eGdXpYSPBBiiFk2QV1J-zLERojcwEurW2tiFJDJxDEF4EB2d3rinQeuAuchIgYlFrIzGY43MbsMx41nuDro2cB9bglN4B7N2bC17ju-DNNs8PlyLK87izNoDD30LMAJnvBxE6CluzdBeB-kdvwXfSZ2e3GXd5786Qh6B3wd20gg_tBUY3bclr4kcMaiIL9cxCAwklph79k-qFpdGK3iEf_kpSXX2q58p82tDiZJIKqA9oaUXzqGCgbsnkTeUPfoPa6_DNLOgeciuA9pHrP5sTh16y4ZToH9LWsKSjdra8rjA265lnC1byTy5juOE0/https%3A%2F%2Fgroups.google.com%2Fd%2Foptout.

--
https://secure-web.cisco.com/10-Q7BscgIuZcDyxU2XAmQaz3dg1kEbY50sAPyctI9NZ3DPQWGvuCGuHr50kuytAWzWxl-hOkXF-KpaGZCP01WLWinkIYQsfbSn_TCBq9eBhavMXgvKrh8U8wl_mKhf6cjtcQqYr1SWMndzkJxuVucwy0cheFkvk6I7XogL5O794izbwfrdR5_Zud68IA-o4sG4GDt4ebSeFj3TNUx6CJYpZwbVmLOCj7p4V_3vuatXBICrjFRaGbdhxPoirHcPz8Ig5DCkSCAMNZStgWr5vsQ0lM9r0rYPKkWnniWzPsbfkTiyiNo-dd5C1azWW2XVu2Z87rjuan4gXx6vhGTvoKWWPErw7KsfPcsv7wqAVH7qY/https%3A%2F%2Fmaterials-welding.blogspot.com%2F
https://secure-web.cisco.com/1LaBBAILJYgmsbnSiKOfNp4ERvxsTdASCAhfAjU3ytDGUYfkr4LT3rCBhTOd9EFLxAIdkwUK8Fkv2JvoEDXqazVSCNlnQj8CdjCU-P82n0uIx7JF2Tsg50IWDNaIkVtsnRWa3pjWZPX6_80IL5rtOnwFZWznAPMd0pasP5sR6goNTJqmQ9ZW5zk5ByYRfNMlluKhP_apveHS2-75mgnbf5_FdO07-rbh5JfMllO-Yiq1dBogPBjSXY0Jw5J1I0Y-_LhuKEdoPGk_WvCtqTY2N14HdbfSII3bhrvjiDNr8Ex63dJmnnB6cH-1O28dws9dBoBi8IC5ooGJfskiretOCkemXLaEBBVKj85cnUf_Jkkc/https%3A%2F%2Fwww.linkedin.com%2Fgroups%2F122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://secure-web.cisco.com/1lAkJPqs7ChEoKdMghq2xCdj16PWJE72RRsw-SXhGHlXXGB9Prd5n7ZubsClw7pm85MGpPdll3-SV656b4j8PV6O-26yogjXLkeu6qgg5H1A57dy91IE6XOHysalcdeljtfnL9grWZiQZeewqG0A5MWJQm_e2it65AkxnyhALPCGJFGo2u-G5cQNDmofoIC4ixLjTIBAjWi7cG2FfyTHOZ-d1gwzAWi0DNewtJNEipQ0oUo_HE5h1xpj0uFuj4Q1gpmyPpeEVyQug4d6a9B6gXC7V0SUjIeT8eJ80KVn4dzIIGudDSmGE-qAuFu3BBQqmp7AT4eL7D-64l9QJvW6h1jv_NGrCw3fro0k-MP90g4k/https%3A%2F%2Fgroups.google.com%2Fgroup%2Fmaterials-welding.
To view this discussion on the web visit https://secure-web.cisco.com/15l9WgdSZFdNyh4lcVOHVbbPxRJSFCgdMMBtv1jkob143nfXRF-HibgJfkUEKFr0IWVXdkAaMCgtGJPKvOnxOw1rMcozyNCcTUpyphapcJhhoC71v8v8m7jkUqvS0ky96S8RPv4mom_HYBIPF_heJCJjlWHZ3ni0hom8iMhHmkvKGC9xjdHlwXbGkM_cXuuP_nuPIweCdnQS9_5OobdmhTnbo3KvKUMSQGbd06c8kb4mHPBkJdnFIq-WhPfuMoobH4aGuEyc_1Nm698Bre9VqYigPDB3CZcFtiR5ynGVWPRswUzEWiU0ClhenvfpuyxRG_qkWv3QAu0r6z0ioQNd78zS6HAmim1ufzcto0BvZKDc/https%3A%2F%2Fgroups.google.com%2Fd%2Fmsgid%2Fmaterials-welding%2FCAEagfUhsC50aqUoYTvyoXMWh9kh_wcL4BX1m3YKjPP_hU9Wdfw%2540mail.gmail.com.
For more options, visit https://secure-web.cisco.com/17ZDQAS8Qh0iUezgzDaXyOBC-ym4sireR_UaTz9PS0LTp88eGdXpYSPBBiiFk2QV1J-zLERojcwEurW2tiFJDJxDEF4EB2d3rinQeuAuchIgYlFrIzGY43MbsMx41nuDro2cB9bglN4B7N2bC17ju-DNNs8PlyLK87izNoDD30LMAJnvBxE6CluzdBeB-kdvwXfSZ2e3GXd5786Qh6B3wd20gg_tBUY3bclr4kcMaiIL9cxCAwklph79k-qFpdGK3iEf_kpSXX2q58p82tDiZJIKqA9oaUXzqGCgbsnkTeUPfoPa6_DNLOgeciuA9pHrP5sTh16y4ZToH9LWsKSjdra8rjA265lnC1byTy5juOE0/https%3A%2F%2Fgroups.google.com%2Fd%2Foptout.

--
https://secure-web.cisco.com/10-Q7BscgIuZcDyxU2XAmQaz3dg1kEbY50sAPyctI9NZ3DPQWGvuCGuHr50kuytAWzWxl-hOkXF-KpaGZCP01WLWinkIYQsfbSn_TCBq9eBhavMXgvKrh8U8wl_mKhf6cjtcQqYr1SWMndzkJxuVucwy0cheFkvk6I7XogL5O794izbwfrdR5_Zud68IA-o4sG4GDt4ebSeFj3TNUx6CJYpZwbVmLOCj7p4V_3vuatXBICrjFRaGbdhxPoirHcPz8Ig5DCkSCAMNZStgWr5vsQ0lM9r0rYPKkWnniWzPsbfkTiyiNo-dd5C1azWW2XVu2Z87rjuan4gXx6vhGTvoKWWPErw7KsfPcsv7wqAVH7qY/https%3A%2F%2Fmaterials-welding.blogspot.com%2F
https://secure-web.cisco.com/1LaBBAILJYgmsbnSiKOfNp4ERvxsTdASCAhfAjU3ytDGUYfkr4LT3rCBhTOd9EFLxAIdkwUK8Fkv2JvoEDXqazVSCNlnQj8CdjCU-P82n0uIx7JF2Tsg50IWDNaIkVtsnRWa3pjWZPX6_80IL5rtOnwFZWznAPMd0pasP5sR6goNTJqmQ9ZW5zk5ByYRfNMlluKhP_apveHS2-75mgnbf5_FdO07-rbh5JfMllO-Yiq1dBogPBjSXY0Jw5J1I0Y-_LhuKEdoPGk_WvCtqTY2N14HdbfSII3bhrvjiDNr8Ex63dJmnnB6cH-1O28dws9dBoBi8IC5ooGJfskiretOCkemXLaEBBVKj85cnUf_Jkkc/https%3A%2F%2Fwww.linkedin.com%2Fgroups%2F122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://secure-web.cisco.com/1lAkJPqs7ChEoKdMghq2xCdj16PWJE72RRsw-SXhGHlXXGB9Prd5n7ZubsClw7pm85MGpPdll3-SV656b4j8PV6O-26yogjXLkeu6qgg5H1A57dy91IE6XOHysalcdeljtfnL9grWZiQZeewqG0A5MWJQm_e2it65AkxnyhALPCGJFGo2u-G5cQNDmofoIC4ixLjTIBAjWi7cG2FfyTHOZ-d1gwzAWi0DNewtJNEipQ0oUo_HE5h1xpj0uFuj4Q1gpmyPpeEVyQug4d6a9B6gXC7V0SUjIeT8eJ80KVn4dzIIGudDSmGE-qAuFu3BBQqmp7AT4eL7D-64l9QJvW6h1jv_NGrCw3fro0k-MP90g4k/https%3A%2F%2Fgroups.google.com%2Fgroup%2Fmaterials-welding.
To view this discussion on the web visit https://secure-web.cisco.com/1ei3LqvvhgQlKklQ_NvRWdJEG1wnIEtRXnXeIKz2YXwFethIbIHJiqiavFfbbPTT0FXvczmvL1YpRhhOxe_ajbTfydRROvtojYa8mR4FC2e-55G9taGEfgZ4QdTc2huNepyrOXO3TtRyUYaQRvQyCvnWnPFNsaJMj6bMJHbKU4NAd4JeUaZVqbE6Sgp4_5IpKda_trOQumQP64Sy-YejpuS6vGqchHXhd5QIT2cWE_kijSxc071qNf4zxrkXM_artW54ue5v4l4Gp9vgkXSUKakWkYT98WSEJdZpa9quOEy2vtW8uh06VvZkdQr8-H441HqtUWyuEUQRNWfBNiq7kMO08klNsdocOxY4CoLC2trk/https%3A%2F%2Fgroups.google.com%2Fd%2Fmsgid%2Fmaterials-welding%2FF1ECCC7A-B6DB-46D4-BB7E-24C1DE3EF4EC%2540gmail.com.
For more options, visit https://secure-web.cisco.com/17ZDQAS8Qh0iUezgzDaXyOBC-ym4sireR_UaTz9PS0LTp88eGdXpYSPBBiiFk2QV1J-zLERojcwEurW2tiFJDJxDEF4EB2d3rinQeuAuchIgYlFrIzGY43MbsMx41nuDro2cB9bglN4B7N2bC17ju-DNNs8PlyLK87izNoDD30LMAJnvBxE6CluzdBeB-kdvwXfSZ2e3GXd5786Qh6B3wd20gg_tBUY3bclr4kcMaiIL9cxCAwklph79k-qFpdGK3iEf_kpSXX2q58p82tDiZJIKqA9oaUXzqGCgbsnkTeUPfoPa6_DNLOgeciuA9pHrP5sTh16y4ZToH9LWsKSjdra8rjA265lnC1byTy5juOE0/https%3A%2F%2Fgroups.google.com%2Fd%2Foptout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/BFE5573062A906469F0CB5F594628E1978774830%40EXCH01.zhi.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...