Hi!
For Monel NiCu7 overlay on CS/LAS no need of any barrier layer you can directly weld NiCu7 on
CS/LAS base as it is comparable while as CuNi7( Cupronickel) is not comparable with CS/LAS) so not recommended to use as barrier layer

Ni1 is used as barrier layer for Monel overlay on CS/LAS for thiner base metal/nozzle pipe to avoid effect of dilution where Fe to be controlled below 2% in undiluted chemistry at closer to the fusion line as possible

Regards
Hegde P.B.

 
On Monday, 22 October, 2018, 12:53:49 PM IST, P.K.Pal <palpk07@gmail.com> wrote:


Due to Fe content problem, whether, it will be better to use ER Cu Ni deposit as barrier layer and then weld deposition with ERNiCu7 ?

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...