Monday, April 23, 2018

Re: [MW:27750] Re: water fill up test after painting of storage tank

I hereby would like to understand what would be the issue if the tank is painted completely ?  Is the water load and pressure will be retained by 500 micron paint , practically ? Think it guys  and correct me if am wrong 

Thanks

On Mon, Apr 23, 2018 at 2:01 PM, Bapat, Ramesh <Ramesh.Bapat@cbi.com> wrote:
Hello Manoj, Sunil Kumar and All

As far as I know,

When the next edition of API 650 is published which is expected to be within the next couple of months, the wording below is to be included to provide guidance to owners who wish to consider internal & external coatings before the tank is hydrotested.  This will be a decision that only the owner can make.

7.3.7.2 Unless otherwise specified by the purchaser, all internal and external coating systems that will cover tank shell joints shall be applied after the hydrostatic test. If specified by the purchaser that a coating system is to be applied to the shell joints before the hydrostatic test, all shell joints to be coated shall be tested in accordance with 7.3.6.2.a prior to the application of coating.

Hope this helps somewhat.

Thanks and Best Regards,

Ramesh



Ramesh Bapat CMfgE, PE
Senior Engineering Advisor (Metallurgy)
Engineering & Construction
ramesh.bapat@CBI.com
CB&I
5850 Rogerdale Road
Suite 225
Houston, TX 77072
www.CBI.com


-----Original Message-----
From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Kumar
Sent: Monday, April 23, 2018 5:51 AM
To: materials-welding@googlegroups.com
Subject: Re: [MW:27745] Re: water fill up test after painting of storage tank

Hi Manoj,

Normally in API 650 tanks water test is done to analyse the settlement & to check leak too.

if the tank internal & external is painted, it may mask any possible pin-holes or cracks etc..

So i personally feel that it is better to do before painting. however expecting experts

opinion on this as well.


Regards,
Sunil kumar

On 4/23/18, pkkanishk2006@gmail.com <pkkanishk2006@gmail.com> wrote:
> Hi Manoj ,
>
> Yes its possible and ok to do a water fillup test after painting , but
> pls ensure that the painting has been given required curing time to
> avoid any cohesive disbandment .
>
> Regards,
> Pratish
>
> On Monday, April 23, 2018 at 3:52:28 AM UTC+1, John Manoj wrote:
>>
>> Dear expert.
>>
>> We have one proposal to do water fillup test after internal and
>> external painting of water tank which is fabricated as per API 650.
>> Internal paint : 300 micron  polyamine cured novolac epoxy coating.
>> External : 205 micron paintining.
>>
>> Is it possible to do water fillup test after painting,
>>
>> Thanks in advance,
>> Manoj.
>>
>>
>>
>
> --
> https://urldefense.proofpoint.com/v2/url?u=https-3A__materials-2Dweldi
> ng.blogspot.com_&d=DwIBaQ&c=j2Bs4Nz3nJdA9D7Jhn4VVQ&r=61Mcn7VrAFeVBk_En
> Yvh6vFn55MRKnZa96lIrbZdZtU&m=RNf_BWqv095Vb8azATMEhf6dUKmqdl-pZOvMQQTdU
> cQ&s=tfVvUIHN521UklvB-R05Te6TiDmZP5YpTkgzhR0QurA&e=
> https://urldefense.proofpoint.com/v2/url?u=https-3A__www.linkedin.com_
> groups_122787&d=DwIBaQ&c=j2Bs4Nz3nJdA9D7Jhn4VVQ&r=61Mcn7VrAFeVBk_EnYvh
> 6vFn55MRKnZa96lIrbZdZtU&m=RNf_BWqv095Vb8azATMEhf6dUKmqdl-pZOvMQQTdUcQ&
> s=XKP_bYfydjf4qbypaJ534FbRC34u61cKeXimOe-FLCk&e=
> ---
> You received this message because you are subscribed to the Google
> Groups "Materials & Welding" group.
> To unsubscribe from this group and stop receiving emails from it, send
> an email to materials-welding+unsubscribe@googlegroups.com.
> Visit this group at https://urldefense.proofpoint.com/v2/url?u=https-3A__groups.google.com_group_materials-2Dwelding&d=DwIBaQ&c=j2Bs4Nz3nJdA9D7Jhn4VVQ&r=61Mcn7VrAFeVBk_EnYvh6vFn55MRKnZa96lIrbZdZtU&m=RNf_BWqv095Vb8azATMEhf6dUKmqdl-pZOvMQQTdUcQ&s=m1EJChqgs29WeWU9KZA7FiNpy7pGgZ9MZ313-rUnwF4&e=.
> For more options, visit https://urldefense.proofpoint.com/v2/url?u=https-3A__groups.google.com_d_optout&d=DwIBaQ&c=j2Bs4Nz3nJdA9D7Jhn4VVQ&r=61Mcn7VrAFeVBk_EnYvh6vFn55MRKnZa96lIrbZdZtU&m=RNf_BWqv095Vb8azATMEhf6dUKmqdl-pZOvMQQTdUcQ&s=-OYNY6JlD1L4-KrFFRB1ciJglETzxuGaRGfgP48LEtQ&e=.
>

--
https://urldefense.proofpoint.com/v2/url?u=https-3A__materials-2Dwelding.blogspot.com_&d=DwIBaQ&c=j2Bs4Nz3nJdA9D7Jhn4VVQ&r=61Mcn7VrAFeVBk_EnYvh6vFn55MRKnZa96lIrbZdZtU&m=RNf_BWqv095Vb8azATMEhf6dUKmqdl-pZOvMQQTdUcQ&s=tfVvUIHN521UklvB-R05Te6TiDmZP5YpTkgzhR0QurA&e=
https://urldefense.proofpoint.com/v2/url?u=https-3A__www.linkedin.com_groups_122787&d=DwIBaQ&c=j2Bs4Nz3nJdA9D7Jhn4VVQ&r=61Mcn7VrAFeVBk_EnYvh6vFn55MRKnZa96lIrbZdZtU&m=RNf_BWqv095Vb8azATMEhf6dUKmqdl-pZOvMQQTdUcQ&s=XKP_bYfydjf4qbypaJ534FbRC34u61cKeXimOe-FLCk&e=
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://urldefense.proofpoint.com/v2/url?u=https-3A__groups.google.com_group_materials-2Dwelding&d=DwIBaQ&c=j2Bs4Nz3nJdA9D7Jhn4VVQ&r=61Mcn7VrAFeVBk_EnYvh6vFn55MRKnZa96lIrbZdZtU&m=RNf_BWqv095Vb8azATMEhf6dUKmqdl-pZOvMQQTdUcQ&s=m1EJChqgs29WeWU9KZA7FiNpy7pGgZ9MZ313-rUnwF4&e=.
For more options, visit https://urldefense.proofpoint.com/v2/url?u=https-3A__groups.google.com_d_optout&d=DwIBaQ&c=j2Bs4Nz3nJdA9D7Jhn4VVQ&r=61Mcn7VrAFeVBk_EnYvh6vFn55MRKnZa96lIrbZdZtU&m=RNf_BWqv095Vb8azATMEhf6dUKmqdl-pZOvMQQTdUcQ&s=-OYNY6JlD1L4-KrFFRB1ciJglETzxuGaRGfgP48LEtQ&e=.
This e-mail and any attached files may contain CB&I (or its affiliates) confidential and privileged information. This information is protected by law and/or agreements between CB&I (or its affiliates) and either you, your employer or any contract provider with which you or your employer are associated. If you are not an intended recipient, please contact the sender by reply e-mail and delete all copies of this e-mail; further, you are notified that disclosing, copying, distributing or taking any action in reliance on the contents of this information is strictly prohibited.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to a topic in the Google Groups "Materials & Welding" group.
To unsubscribe from this topic, visit https://groups.google.com/d/topic/materials-welding/8By4YsqP54M/unsubscribe.
To unsubscribe from this group and all its topics, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...