Wednesday, January 18, 2017

Re: [MW:25924] PWHT Cycle Of P335-P5B (P9)

u have to keep below Mf temp for sufficient time to form tempered martensite say below 120 degree celsius

THANKS & BEST REGARDS,
KG.PANDITHAN, IWE,  AWS-CWI, CSWIP 3.1,
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349

On Tue, Jan 17, 2017 at 8:18 PM, dilintas <dilintas@gmail.com> wrote:
Boxbe This message is eligible for Automatic Cleanup! (dilintas@gmail.com) Add cleanup rule | More info

You have to allow martensite to formally and at the same time avoid cold cracking. Therefor keep the 200 degC for 2 hours and then proceed as you propose



Sent from my Samsung Galaxy smartphone.

-------- Original message --------
From: 'Mostafa Kamel Hussein' via Materials & Welding <materials-welding@googlegroups.com>
Date: 17/01/2017 11:40 (GMT+02:00)
To: Materials-welding <materials-welding@googlegroups.com>
Subject: [MW:25910] PWHT Cycle Of P335-P5B (P9)

Dear Sir
Really now we are in critical situation regarding PWHT of A335 - P5B (Grade P9). The cycle in brief as attached. first preheat at 200°C then cooling to ambient temperature (20-80°C) for minimum 30 minutes as holding time. after that PWHT cycle starts by heating rate of maximum 100°C /hr till reaching to soaking temperature (704-760°C) for 2hrs. finally, cooling rate of maximum 100°C /hr.
My question is: it this PWHT cycle for P335-P9 true specially cooling to ambient temperature (20-80°C) as i know it's may cause delay crack?
and if this cycle wrong, can you provide me with the correct one which i can built PQR on it?

Your quick reply is highly appreciated.

Regards,
Mostafa K

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/i45flf0ykah0c0samsynqpwi.1484664522517%40email.android.com.
For more options, visit https://groups.google.com/d/optout.


--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJzm4ePWpX6ndnevKC2iD%3DMY-xJ7FnA91owattiiu7sxAZMyxQ%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...