Dear Mr. Shah,
First you have to purchase electrodes as per the your specified requirment.
In addition to the above, for achieving this you have to take care for following:
1. No filing/ brushing/ grinding etc. should be done on welds before measuring ferrite %
2. Allow weld to cool in open air
3. The ferrite should be measured immediately after cooling of the welds
Best Regards,
Rajnish
--------------------------------------------
On Fri, 5/20/16, SATISH SHAH <sbdr1912@gmail.com> wrote:
Subject: [MW:24816] Ferrite % 4-8 of E309LMo
To: "Materials & Welding" <materials-welding@googlegroups.com>
Date: Friday, May 20, 2016, 3:49 PM
Dear Expert,
Let me know Ferrite 4 - 8 % is possible to obtain of
Electrode 309LMo as weld condition.
Regards
SATISH SHAH
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members
personel views and meant for educational purposes only,
Users must take their own decisions w.r.t. applicable
code/standard/contract documents.
---
You received this message because you are subscribed to the
Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails
from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/8c7f5e73-c5e0-4c60-ab4f-92cb2537713b%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/1960327134.1201241.1466430002179.JavaMail.yahoo%40mail.yahoo.com.
For more options, visit https://groups.google.com/d/optout.
Subscribe to:
Post Comments (Atom)
[MW:35692]
Dear all Can I do MPI above painting surface for cs tank Regards, Sriram Srinivasan -- https://materials-welding.blog...
-
Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? ...
-
Definition of buttering from ASME Section IX, QW/QB-492 Definitions: Buttering: the addition of material, by welding, on one or bot...
-
Section I. PRINT READING 3-1. GENERAL a. Drawings . Drawing or sketching is a universal language used to convey all necessary information to...
No comments:
Post a Comment