[MW:25039] RE: 25036] RE: 25027] impact results - UHT material welding

Hi Fernando,

 

Welding of 517 grades is never easy. It becomes difficult when impact properties are in question. If you could share details about (MTR) the materials, welding consumable, and the failed PQR, then there could be some meaningful suggestions provided.

 

Thanks.

 

 

 

Pradip Goswami, P.Eng,IWE
Independent Welding & Metallurgical Engineering Specialist ,
Ontario,Canada.
ca.linkedin.com/pub/pradip-goswami/5/985/299

pgoswami@quickclic.net

pradip.goswami@gmail.com

 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Alan Denney
Sent: Thursday, June 30, 2016 4:43 AM
To: materials-welding@googlegroups.com
Subject: [MW:25036] RE: 25027] impact results - UHT material welding

 

There is an assumption here that the weld as deposited met the certificate values which reduced as a result of the PWHT. I don’t expect that you had anything like the certificate results in your weld as-welded. Was it tested in the as-welded condition for comparison purposes? Normally PWHT would improve the results (not always though – because you are into the finer points of the weld metallurgy here). It is the way the weld has been deposited which gave the poor results, not what that consumable can achieve when deposited under ideal conditions.

 

Alan Denney

AKD Materials Consulting Ltd

 

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Fernando L Neto
Sent: 29 June 2016 20:00
To: materials-welding@googlegroups.com
Subject: [MW:25027] impact results - UHT material welding

 

Dear colleagues, 

 

I hope this email finds all you well

 

Project: ASME VIII- Pressure vessel - material ASME SA517 Gr B. Thickness 9,5 mm.

 

 I have to qualify a WPS for welding ASME SA517 - B with impact requirements at -40 C, 

 

Also is required PWHT, and my first results of impact test @-40C of test plate were very low. (lateral expansion less than 0,2mm and energy less than 20J)

 

The declared Values of certificate of consumable is 75J @ -73C  !!!

 

Can the presence of PWHT changes so much the values of impact test? (certificate´s value is "as welded" and my results is "after PWHT".

 

Any help will be very useful. 

 

Thanks a lot, 

 

Fernando Lescovar Neto (IWE)

 

 

 

 

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CANv%2BETZM4c_%3Dh%2BeKOosPusHUqGE_5b0DZ3aO12GyNDPph3dUbw%40mail.gmail.com.