Friday, April 17, 2015

RE: [MW:23124] Change of Brand for SAW Consumables

To Everyone in Welding and Materials Community,
 
This query has generated many responses, many just on the fly some are detailed. SAW is a key welding process for any good fabrication related work. FLUX is the key to any SAW process, more than filler wire. Hence a change of flux is considered as an essential variable.
 
Wire flux classification test is done by manufacturers in undiluted test pads or groove joints (see SFA 5.23). Those results vs. the the PQR results differs in many instances, due to dilution ,heat input........etc.
 
Hence if the flux is changed the PQR should be prequalified.
 
ASME interpretations are one or two lines, many be a short paragraph with a lot of inner meanings.
 
Perhaps a spread sheet with all the pro and the cons would be beneficial to all.
 
Also I would like to say the question is open ended. If one is asking an engineering solution, design code, specifications, technical requirements all needs to be considered, which is missing for many queries off late.
 
Thanks.
 
 
Pradip Goswami, P.Eng,IWE
Welding & Metallurgical Engineer/Specialist
Ontario, Canada
 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Jim Price
Sent: Friday, April 17, 2015 7:59 AM
To: materials-welding@googlegroups.com
Subject: RE: [MW:23123] Change of Brand for SAW Consumables

PQRs are welded to filler metal and flux classifications not brand names.

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Kannayeram Gnanapandithan
Sent: Friday, April 17, 2015 1:16 AM
To: materials-welding
Subject: Re: [MW:23121] Change of Brand for SAW Consumables

 

No in classicification, only brand name is changed which is not essential for no impact requirements. It can be used

On 17-Apr-2015 11:02 am, <george.dilintas@gr.bureauveritas.com> wrote:

This interpretation is too old.
Please refer to the latest edition of the Code Section IX - QW 404.35

best regards

Dr. Georgios Dilintas

Authorized Nuclear Inspector
Authorized Inspector Supervisor

I&F REGIONAL TECHNICAL MANAGER
BUREAU VERITAS PIRAEUS - GREECE

Tel: +30 210 40 63 113 /4 /5
Fax: +30 210 40 63 118
Cell: +30 69 44 64 62 04


Gurunathan R ---16/04/2015 17:28:46---Please refer the interpretation below. Status:  Currently Valid

From: Gurunathan R <saneguru@gmail.com>
To: Materials-Welding <materials-welding@googlegroups.com>
Date: 16/04/2015 17:28
Subject: Re: [MW:23116] Change of Brand for SAW Consumables
Sent by: materials-welding@googlegroups.com





Please refer the interpretation below.


Status:  Currently Valid
Other Links:
________________________________________________________________________________   
Interpretation:    IX-83-169
Subject: Section IX, QW-404.9
Date Issued: May 14, 1985
File: BC85-089

Question: For submerged-arc welding, can a fabricator use a different brand of flux than that specified in a wire-flux classification for which he is qualified, without performing a new PQR?

Reply: No.


Best Regards,
Gurunathan.R

On Wed, Apr 15, 2015 at 5:22 PM, Mhaskar Aly <mhaskar.aly@gmail.com> wrote:


Dear All,
We have PQR of following details:

 

Process SAW with Filler Wire EM12K (ESAB) with Flux F7A8 (ESAB OK 10.62 Flux)

 

Question:
1.       Can we use Filler Wire EM12K (Bohler) with Flux F7A8 (ESAB OK 10.62 Flux)
2.       Can we use Filler Wire EM12K (Bohler) with Flux F7A8 (Bohler Flux)

 

Kindly advise as per ASME Sec IX…with reference.

 

Thanks in advance

 

Thanks & regards

 

Ali Mhaskar,

QA/QC Manager

Velath Engineering International FZC; Hamriyah FreeZone Sharjah, UAE; * P.O Box 6268 – Sharjah UAE.
(
Phone: 00971-6-526 9269, 526 9185, 526 9119 Ext-212 ÈMobile no.: 00971-55 265 3598 ÊFax no. 00971-6-526 9393  üwww.velath.com

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to
materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to
materials-welding@googlegroups.com.
Visit this group at
http://groups.google.com/group/materials-welding.
To view this discussion on the web visit
https://groups.google.com/d/msgid/materials-welding/CAOenW4htWh-B5O0xAn_yPAbYpWWRcX6NWmDT5tmmziG3jgPAxQ%40mail.gmail.com.
For more options, visit
https://groups.google.com/d/optout.

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CACt3NQMvdpRSdPy5%3DYtKhQPuHW58N8oxHWbeaP6xnSqws%3DC3Sg%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

This message contains confidential information. To know more, please click on the following link: http://disclaimer.bureauveritas.com

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/OF638A3179.D4435A26-ONC2257E2A.001E5636-C2257E2A.001E6C88%40LocalDomain.
For more options, visit https://groups.google.com/d/optout.

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJzm4eOh4j3xJpqLnuwCgFyUqUaAMiSsdECDgGBU%3D9eqsG_iQw%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/029c9b90d0414321b81a483691f9daec%40POLARMAIL.PolarTank.local.
For more options, visit https://groups.google.com/d/optout.

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...