Hi Silambarasan ,

If the welding is for ASME Sec VIII Div -1 Vessel, then test Macro ( for MLP check ) , PT, Visual. This is enough as per ASME-IX QW - 193 requirements.

Hardness & RT are Special Tests as per Client requirements only, inorder to judge the hardness value . Quite Stringent too.

Pull out & Tear tests are required for Sec VIII , Div-2 Vessels, If I am not mistaken.

Do you have Client Spec to weld this MockUp ?

Read again ASME-IX,  QW 193. 1 to 3 for MockUp testing requirements and you must read QW-288 for Essential Variables to follow during Qualification.

Regards,
Saravanan

 

On Mon, Jan 12, 2015 at 2:55 PM, silambarasan veluchamy <chimbu.shawn@gmail.com> wrote:
Dear members,
We are going to carry out a Mockup Procedure qualification for T-TS joint as per ASME SecIX. what are the test required to carry for the qualification. I hear from a TPI that RT, Tear test & pull out has to be carried out, whereas ASME Sec IX & Tema class 'R' are not talking about the above said tests. 
Is the above said tests required? If so, the as per which standard?
Kindly advice

BR,
M.V.Silambarasan

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/eb910586-77a2-4489-a880-880f18dbb748%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CALV1rk%2BC3ZUVHoWdkuRrkNJawQB_h8H58zgF7wENXOyA5GtTXQ%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...