As our dear friend, Mr. Henning mentioned, longitudinal bend is useful when testing weld metal or base metal combinations which differ markedly in bending properties. That's absolutely true...

I know from experience that in these cases, bend specimen may not "bend" as we want it to. This means that the weld may not be at the center of bent specimen where it should be.The specimen slips and normally, the weld area (weld + H.A.Z.) will not be at the center of bend and your bend test will not be valid...!!!

 Guided bend test helps but still, you need a skilled operator or maybe you do not have access to guide bend test apparatus. 

On the other hand, longitudinal bend test does not need any of these and with a simple apparatus, you will have a nice bend test. This becomes important when you are dealing with a critical weld and need to careful and critical. Just do not forget to prepare a large test coupon...!!!

Best Regards

Ramin Kondori

Sr. QA/QC engineer

Yadavaran Oilfield Project

SIPC (SINOPEC)



On Wed, Apr 23, 2014 at 7:16 PM, John Henning <jhenning@deltak.com> wrote:

Refer to QW-161.5,  to whit:

 

"Longitudinal bend tests may be used in lieu of the transverse side-bend , face, and root bend tests for testing weld metal or base metal combinations which differ markedly in bending properties between  (a) the two base metals, or (b) the weld metal and the base metal."

 

John A. Henning

Welding & Materials

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Avinash Pandey
Sent: Wednesday, April 23, 2014 1:25 AM
To: materials-welding@googlegroups.com
Subject: [MW:20651] Reg:Longitudinal tensile and bend test

 

Dear All

 

1. I have a query regarding transverse bend test and longitudinal bend test mention in ASME sec.IX.

2.when to use these test  for procedure qualification.

 

Regards 

Avinash Pandey

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.


______________________________________________________________________
The information in this email is confidential, and is intended solely for the addressee(s). If you are not the intended recipient of this email please let us know by reply and then delete it from your system; you should not copy this message or disclose its contents to anyone. The internet can not guarantee the integrity of this message. HAMON (and its subsidiaries) shall (will) not therefore be liable for the message if modified.
______________________________________________________________________

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...