[MW:18457] RE: 18456] Re: May E8018-C1 substitue E8018-G to weld Corten Steel

Hi Abuzar,
 
The default electrodes for these grades of steel is E-8018-W2/W1. However some electrode manufacturers may market this product under "G" classification. As per ASME Sec II part C, the "G" classification should meet the nominal chemistry in  specified in SFA 5.5.The additional alloying elements are acceptable  subject to mutual agreement between the manufacturer and the user.
 
If E-8018-G matches the chemistry of E-8018W2(for Corten -B) and E-8108-W1(for Corten-A), then the deviation may be allowed. You have  to compare the MTR's of both types of electrodes to arrive at a conclusion.
 
 
Thanks 
 
Pradip Goswami, P.Eng,IWE
Welding & Metallurgical Specialist
Ontario, Canada
 
 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Abuzar Malik
Sent: Saturday, August 17, 2013 8:35 AM
To: materials-welding@googlegroups.com
Subject: [MW:18456] Re: May E8018-C1 substitue E8018-G to weld Corten Steel

Hi everyone. i am also facing the almost same issue. we are short for E 8018 W2 electrode for corten steel. now contractor wanted to use  E 8018 G electrode as a W2 replacement. kindly guide me whether to allow him or not? reply kindly?

On Thursday, 20 October 2011 14:16:58 UTC+5, Tunisian Quality Engineer wrote:

Hi all

For welding Corten steel, we have in storage E8018-C1 Electrod, may it substitue  E8018-G, how can confirm ?

Regards
--
زكرياء غراب
GHRAB Zakaria
مسؤول عن الجودة
QA/QC SENAD
مشروع المحطة الحرارية ـ الوحدة الرابعة
المحمدية ـ المغرب

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...