Re: [MW:16596] Linier indications observed in Radiography Testing in SA240 310S weld

Hi
 
No need to preheat.
Such microfissures are often encountered while welding 310 grade.
 
Control your Interpass Temperature strictly while welding. Also weld with higher travel speeds to minimise your heat input.
 
Regards
 
Prem Nautiyal


--- On Wed, 1/23/13, mukesh.chaudhari <mukesh.chaudhari@orientalindia.net> wrote:

From: mukesh.chaudhari <mukesh.chaudhari@orientalindia.net>
Subject: [MW:16580] Linier indications observed in Radiography Testing in SA240 310S weld
To: materials-welding@googlegroups.com
Date: Wednesday, January 23, 2013, 4:41 PM

Dear Expert,

We are doing SA240 Type 310s material welding with WPS(GTAW) but there are lot of defects of linier indications(micro cracks) observed in Radiography testing.

We are using D&H make ER-310 filler wire for welding. We also preheat the joint up to 80 °C to avoid sudden cooling.

Can you guide me how to avoid linier indications(micro crack) in welding.

 

Regards,

Mukesh

 

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...