AST M A 514  is a high-strength quenched and tempered plate for structural and pressure vessel applications.
It is also known as US T-1 steel.  Consumables used are:

SMAW              A 5.5                 E 11018 M / E12018 M
GMAW             A 5.28                ER 110S-1 / ER 120 S
FCAW              A 5.29                E 11XT1-K3C / K3M (or) E 11X T5-K3C / K3M

Stop the weld if required  and don't do continuous welding.
Maintain max. inter pass temp. to 120 deg. C.

Sridhar.
 
---------------------------------------------------------------------------------------------------------------------------------------------------------------------
 From: hany alfy <hanyon_alfy@yahoo.com>
To: "materials-welding@googlegroups.com" <materials-welding@googlegroups.com>
Sent: Wednesday, 30 January 2013 1:06 PM
Subject: [MW:16635] ASTM A514 TYPE T-1



Dear All

We need to fabricate one mechanical Grab plates are grade ASTM A514 TYPE T-1
Which electrode we can use for welding

Regards,
H.A
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 


No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...