Dear Sir,

 

I don't know what ASME says about PWHT but in the EN 10028-3 there is a warning about PWHT for this material regarding holding time and/or temperature (see paragraph 8.2.4 of EN 10028-3). When the outcome of following formula comes above 17,3 there is a risk that the material properties will be reduced and no longer met the requirements of the specification.

 

P = Ts (20 + lg t) x 10-3

 

Where Ts = PWHT temperature in °K and t is holding time in hours

 

If your outcome is above this 17,3 than you need to prove that all mechanical properties still meet the requirements by simulating PWHT on a sample from the same heat and thickness as used for your pressure vessel.

When executing more than one PWHT than you should calculate the value for each separate treatment and look at the sum of all treatments together.

Keeping this formula in mind you also can calculate any possible heat treatment conditions (temperature for thickness of 14,3 max. 630 °C)

 

Met vriendelijke groeten / Best Regards

 

Herman Pieper

 

Pieper Quality Support & Inspection

Phone: +31 (0)521 380083

Fax:     +31 (0)84 7539225

Cell:     +31 (0)6 51691215

www.pieper-qsi.nl

 

Van: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] Namens David Stevenson
Verzonden: dinsdag 27 september 2011 23:27
Aan: materials-welding@googlegroups.com
Onderwerp: [MW:12563] PWHT of modified P460 NL1 (1.8915) EN 10028-3

 

As this material is not in the tables can anyone provide the PWHT process for material 14.60mm thick in a pressure vessel built to ASME section VIII division 2?

 

THE FIRST CHOICE IN TANK CONTAINERS

DAVID STEVENSON
TECHNICAL MANAGER
Eurotainer U.S. INC.
5810 Wilson Rd. Suite 200, Humble, Texas, 77396 USA
Phone 01 832 300 5019 (Direct)● Mobile 01 713 805 0192 ● Fax 01 832 300 5050

email: dstevenson@usa.eurotainer.com ● website: www.eurotainer.com

 Please consider the environment before printing this document

 

--
To post to this group, send email to
materials-welding@googlegroups.com
To unsubscribe from this group, send email to
materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...