First idea is to use CrMo2 consumables (or CrMo1 could be solution too, depending on application / requirements)

Preheat 200 degrC

PWHT at 690 °C , however

·         PWHT temperature is depending on strength requirements 4130 and required charpy values in weld metal

·         duration is depending on wall thickness and required charpy values in weld metal

 

Stick electrodes

·         OERLIKON CROMOCORD 2 STC

·         OERLIKON OE KV3 HR

TIG rod:

·         OERLKON CARBOROD CrMo2  or

·         OERLIKON CARBOROD KV3 (=B2)

 

Erwin Gering

AIR LIQUIDE WELDING

OERLIKON_RVB_5cm.BMP

 

Van: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] Namens rajagopal kannan
Verzonden: woensdag 28 oktober 2009 8:23
Aan: materials-welding@googlegroups.com
Onderwerp: [MW:3559] CONSUMABLES

 

Dear Members,

Could you please suggest me the apt consumable for GTAW and SMAW to weld SA 182 Gr. F22 cl.1 with AISI 4130?

Thanks and Best Regards,

K.Rajagopal



--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...