[MW:1818] RE: 1804] 410 weld overlay on SA 516 Gr 70

Yes. We have tested several SS 410S PQRs and cleared the side bend tests.
Have you tried bend test so far. If it is failing which area you are getting
openings, is it on the corners of the overlay to CS junction. Or in the
middle of overlay area ? If it is on the corners, you need to
1) round off the corners with 2-3mm radius,
2) merge / Blend toes of the overlay passes to the CS base metal

Regards.

C. K. Purohit
General Manager - QC
KNM Process Systems Sdn Bhd - Malaysia

HP No. : 6016-3376448
-----Original Message-----
From: materials-welding@googlegroups.com
[mailto:materials-welding@googlegroups.com] On Behalf Of JASPAL SINGH
Sent: Wednesday, March 25, 2009 4:52 PM
To: Materials & Welding
Subject: [MW:1804] 410 weld overlay on SA 516 Gr 70


Is it possible to clear the bend test in SS410 weld overlay. The
barrier layer is E309LMo .
if possible let me know how.

Jaspal Singh
919996624244

<FONT FACE="Arial">
<B>***DISCLAIMER NOTICE ***</B><BR>
"This email and any files transmitted with it is confidential and is intended only for the use of the recepient(s) named above. If you are not the intended recipient, any review, retransmission, dissemination, distribution, printing, copying or use the information contained in this message or any part thereof in other manner is strictly prohibited. If you receive this email in error, please notify the sender immediately by return email and delete the email and any of its attachments. Any personal views or opinions expressed by the sender shall be understood as neither given nor endorsed by KNM or any of the companies within the Group."
<BR>
</FONT>

--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...