EN8 which is having high carbon content (upto 0.44%) and CE in excess
of 0.45 needs preheating 100-150 deg.C
use low hydrogen eletrodes and PWHT to avoid hardening and cold
cracks.

you might try establishing PQR with the above.

On May 17, 3:43 pm, "PREM SHANKARDUTT NAUTIYAL"
<prem_nauti...@rediffmail.com> wrote:
>
> Dear Friends
>
> Can anyone tell whcih SMAW electrode to use to weld EN8 to SA516 Gr.70 and EN24 to SA 516 Gr.70.
>
> Both are butt joints around 50mm thk.
>
> Regards
>
> Prem Nautiyal
>
> PREM S NAUTIYAL
> CELL : 9820313278
--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...