Saturday, September 1, 2007

CHROME-MOLY and the EMBRITTLEMENT FACTORS

A major application of 2.25% Cr- 1.0% Mo steels is in the fabrication of pressure vessels to be used in oil refining operations where the materials are subjected to elevated temperatures for extended periods of time. Due to this long term exposure, a phenomenon known as temper embrittlement has a tendency to occur. Temper embrittlement is the migration of certain elements within the material to the grain boundaries over time, causing a loss in toughness. As a means to judge the relative temper embrittlement resistance of a material, the so called x- and J-factors were developed.

The J-factor was originally developed for the base materials and incorporates the elements Manganese, Silicon, Phosphorous and Tin in the following formula:

J = [ ( Mn + Si ) x ( P + Sn ) ] x 104

where the various elements are expressed in wt %. Most common specifications call for a J-factor of less than 150 but values as low as 120 have been seen. The control of these elements in the base material is critical since the Mn and Si tend to cosegregate with the P and Sn to cause the loss in toughness.

For the weld metal, the J-factor is not suitable since the rapid solidification and cooling rate of the weld beads do not allow time for the cosegregation of the Mn and Si. In fact, both Mn and Si are needed in the weld metal system; the Mn to develop the needed toughness and the Si for weldability.

Therefore, the x-factor was developed as a better means to judge the relative temper embrittlement resistance of the weld metal by incorporating the residual elements Phosphorus, Antimony, Tin and Arsenic as follows:

x = 10 P + 5 Sb + 4 Sn + As

100

where the elements are expressed in ppm. Typical specifications currently call for a maximum x-factor of 15. This calculation has proven much more effective in gauging the temper embrittlement resistance of the weld metal by controlling those elements that tend to affect the toughness the most while not considering Mn and Si due to the inherent differences in the steel and weld metal.

To meet the requirements for temper embrittlement resistance as currently seen in engineering specifications, the following Thyssen consumables can be used:

A387 Grade 11 and similar 1.25% Cr - 0.5% Mo Steels:

Thyssen Brand S2CrMo / UV420TTR SAW Wire / Flux

Thyssen Brand Chromo 1 Coated Electrodes

A387 Grade 22 and similar 2.25% Cr - 1.0% Mo Steels:

Thyssen Brand S1CrMo2 / UV420TTR SAW Wire / Flux

Thyssen Brand Chromo 2 Coated Electrodes

Test reports and technical papers are available upon request that outline in greater detail the phenomenon of temper embrittlement and its control, including additional specification requirements, optimization of filler metals, and the results of mechanical tests.

http://www.btwusa.com/html/ppf8.html

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...