Hi
Heat treatment of a explosion bonded plates can be done. There wont be any problem with respect to precipitation.  We have done SA 516 gr 70 + 316 L plate nd we have done it for higher thickness plates where the base is 85 +3 mm clad nd after final fabrication the vessel is pwht. Thickness lower than 40 mm will need pwht after explosion bonding since to improve the tensile values and remove the stress due to explosion bonding. The heat treatment after explaosion will be based on the thickness nd to a max of 30 min to 45 min. 

Regards

Nitin Shetty


Sent from Samsung Mobile



-------- Original message --------
From: nishant nair <nishant852003@yahoo.com>
Date: 30/09/2013 21:09 (GMT+04:00)
To: materials-welding@googlegroups.com
Subject: Re: [MW:18819] Clad plate heat treatment as per SA 264 after explosion bonding


Hi there Mr. Krishna,

Well as far as the heat treatment is concerned no deviation from d standard should be accepted. So please be firm on that account if applicable.

Explosion bonded plates can be separately heat treated before explosion bonding and which I think is a feasible option. Reason I think is due to difference of heat treatment procedures of two different metals i.e. annealing and normalizing. This is accepted by SA264 standard also. Pls go through.

Nothing is mentioned regarding the heat treatment of explosion bonded plate in the standard.

Thanks and regards,
Nishant Nair

Sent from Yahoo! Mail on Android



From: george.dilintas@gr.bureauveritas.com <george.dilintas@gr.bureauveritas.com>;
To: <materials-welding@googlegroups.com>;
Subject: Re: [MW:18817] Clad plate heat treatment as per SA 264 after explosion bonding
Sent: Mon, Sep 30, 2013 12:30:00 PM

The issue is the following:

The explosion bonding process will affect the properties of the 304 austenitic s.s?

With other worlds: the explosion bonding will lead to a precipitation of the chromium carbides and therefore a solution annealing heat treatment will be necessary to get a solution of those carbides in the 304 matrix?

Can your material manufacturer guarantee the properties of 304 without heat treatment?

Could you ask for the parameters of the explosion bonding process?
Could your manufacturer give you the temperatures which develop during this process and the relevant time periods?

 

    best regards

    Dr. Georgios Dilintas

    Authorized Nuclear Inspector
    Authorized Inspector Supervisor
    API 510 Inspector
    Prelude FLNG ASME Subject Matter Expert

    I&F REGIONAL TECHNICAL MANAGER
    BUREAU VERITAS HELLAS

    Tel: +30 210 40 63 113/4
    Fax: +30 210 40 63 118
    Cell: +30 69 44 64 62 04
    Korea cell phone: +82 10 2777 8922

Inactive hide details for krishna mudhale ---27/09/2013 19:36:38---Dear experts, Please clarify our issue ie. In our case clad krishna mudhale ---27/09/2013 19:36:38---Dear experts, Please clarify our issue ie. In our case clad plate(SA 387 Gr.11

From: krishna mudhale <kmudhale@gmail.com>
To: materials-welding@googlegroups.com
Date: 27/09/2013 19:36
Subject: [MW:18785] Clad plate heat treatment as per SA 264 after explosion bonding
Sent by: materials-welding@googlegroups.com




Dear experts,
Please clarify our issue ie. In our case clad plate(SA 387 Gr.11
Cl.1+SS 304L), as per our customer spec.  Heat treatment of the clad
plate shall be as per applicable clad plate material specification
ie.SA 264 . But our clad plate manufacturer insists that for higher
thickness clad plates heat treatment is not required(ie.46,54,75Thk) &
for lower thickness he will perform heat treatment(ie.24&28Thk). So my
question is as per SA 264 is heat treatment is required or not for
clad plates after explosion bonding and if required which type of heat
treatment is required.
Please clarify my query & thanks in advance for your valuable feedback.
--
With Warm Regards
Krishna Mudhale

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit
https://groups.google.com/groups/opt_out.

This message contains confidential information. To know more, please click on the following link: http://disclaimer.bureauveritas.com

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

No comments:

Re: [MW:34913] Filler wire

E71T-1C  is Charpy Impact tested at -20degC E71T-1CJ is Charpy impact tested at -40degC. AWS Classification for FCAW is only a supplementary...