Tuesday, April 2, 2013

Re: [MW:17272] RE: 17261] Welding of E316L material -Reg

As per SFA 5.9,   C is max .03% for ER 316L,, in this case what should be done?

Pandithan
Welding Consultant


On Tue, Apr 2, 2013 at 8:14 AM, pgoswami <pgoswami@quickclic.net> wrote:
Hi Siva,
 
If the intended service for S.S 316L is for corrosive environments , then the answer is NO.
 
Like base metals , welding consumables for SS 316 could be manufactured as "Dual Certified Grades". Example as per SFA 5.4
  • For E-316-XX-- Maxm "C" allowed is -0.08%
  • For E-316L-XX-- Maxm "C" allowed is -0.04%
If the electrode manufacturer " Restricts C to  0.04%, yet the  all mechanical test as per SFA 5.4  are passed, then  this grade could be certified as "Dual Certified Grade" , e.g -  E316/E316L-XX. Please check this point with electrode supplier. If the answer is yes then welding consumable certified as  E316/E316L-XX, are safe to use for welding S 316L.  However the consumable must meet any corrosion test, say ASTM A-262 Practice E, if required.
 
Hope this will guide you well to cope with the problem.
 
Thanks.
 

Pradip Goswami,P.Eng.IWE

Welding & Metallurgical Specialist

Ontario, Canada.

Email-pgoswami@sympatico.ca,

pgoswami@quickclic.net

 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of siva subramanian
Sent: Monday, April 01, 2013 11:02 AM
To: materials-welding@googlegroups.com
Subject: [MW:17261] Welding of E316L material -Reg

Dear sirs,
                 I have one clarification regarding welding of SA240 GR 316L material.
May I use E316-16 to weld 316L material.If it is not possible means What is reason behind?

Please Clarify me.

Always Thankful,
A.Sivasubramanian

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

No comments:

[MW:34916] Applicability of Impact requirement as per ASME B31.3

Dear All, Design code – ASME B31.3, Welding Code- ASME BPVC SEC IX Material  to be used used during Fabrication - SA 333Gr6 (P No.1 G...