For Local PWHT of P91, Induction Heating is best method compare to
Resistance pad heating as temp diff is more in Resistance heating and
also ensure that it does not cross over 775 degree celsius
we have done lot on P/T91 from thick 6mm to 60 mm
Pandithan
Welding Consultant
On 2/13/13, Chinnapureddy Kotireddy <chinnapureddykotireddy@gmail.com> wrote:
> Dear Sandeep,
> I have also got similar problem
> By using induction heating for PWHT of p91,There is a huge difference
> between the temp of ID and OD.
> Kindly share your experience and suggestions so that it may benefit us to
> proceed furthur in PWHT of p91
>
> koti
> cell:9486575298
>
> --
> To post to this group, send email to materials-welding@googlegroups.com
> To unsubscribe from this group, send email to
> materials-welding+unsubscribe@googlegroups.com
> For more options, visit this group's bolg at
> http://materials-welding.blogspot.com/
> http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
>
> The views expressed/exchnaged in this group are members personel views and
> meant for educational purposes only, Users must take their own decisions
> w.r.t. applicable code/standard/contract documents.
> ---
> You received this message because you are subscribed to the Google Groups
> "Materials & Welding" group.
> To unsubscribe from this group and stop receiving emails from it, send an
> email to materials-welding+unsubscribe@googlegroups.com.
> For more options, visit https://groups.google.com/groups/opt_out.
>
>
>
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
Subscribe to:
Post Comments (Atom)
Re: [MW:34874] ASME IX, groove weld during WQT limits for Fillet Weld production
Hi David, There are two points in WQT. 1. Thickness of Base Metal -T 2. Thickness of Weld Metal -t When you use a combination of two proces...
-
Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? ...
-
Definition of buttering from ASME Section IX, QW/QB-492 Definitions: Buttering: the addition of material, by welding, on one or bot...
-
Section I. PRINT READING 3-1. GENERAL a. Drawings . Drawing or sketching is a universal language used to convey all necessary information to...
No comments:
Post a Comment